Metal Oxide Varistor: Pure Zinc Oxide at 1400 °C, Bismuth Oxide Paste Fired at 800 °C (Masuyama 1972, Ex. 4)
A varistor made the other way round: a disc of pure zinc oxide, sintered, with bismuth oxide fired into its faces from a paste instead of mixed in. Sintered at 1400 °C and fired with the paste at 800 °C, the disc measured a C-value of 85 at 1 mA and a nonlinearity exponent n of 7.2. Masuyama found that firing on the bismuth oxide paste raises n a great deal over mixing it in.
Source: T. Masuyama, M. Matsuoka and T. Nishi (Matsushita), US 3,663,458 (1972), Example 4. Unknown: how the aluminium is sprayed on, what the silver paint is, and how strong the epoxy solution of the paste is. The 10 g batch is our arithmetic. Picture: the patent's drawing.
མཐོ་རིམ
2 days
ལམ་སྟོན
1
1
Press pure zinc oxide at 340 kg/cm²
Press pure zinc oxide at 340 kg/cm²
Press zinc oxide powder at 340 kg/cm². Example 4 gives no disc size; ours: discs 13 mm across and 2.5 mm thick in the mould of Example 1.
གོམ་པ་འདིའི་རྫས་རིགས:
ཟིངཀ་ཨོག་སའིཌ་ཕུད་རྡུལ1 as requiredལག་ཆས་དགོས་མཁོ:
ལག་པ་འདྲ་མཉམ་གྱི་སྲང་།
ཧའི་ཌོ་ལིཀ་ནོན་འཕྲུལ།
སྡེར་ཆས་ནན་བཙིར་གྱི་ དཔེ་ཚད།
བར་ནི་ཡར་གྱི་འཇལ་ཆས།2
2
Sinter 1 hour at 1400 °C and cool
Sinter 1 hour at 1400 °C and cool
Heat the pressed disc for 1 hour at 1400 °C, then let it cool to room temperature.
ལག་ཆས་དགོས་མཁོ:
མཱཕལ་ཐབ3
3
Lap both faces
Lap both faces
Lap both faces with silicon carbide abrasive. Example 4 gives no thickness.
ལག་ཆས་དགོས་མཁོ:
བར་ནི་ཡར་གྱི་འཇལ་ཆས།4
4
Coat with bismuth oxide paste and fire at 800 °C
Coat with bismuth oxide paste and fire at 800 °C
Coat both lapped faces with a paste of 50 % by weight bismuth oxide in a solution of epoxy resin in butyl alcohol, and fire it in air at 800 °C for 30 minutes. The bismuth oxide diffuses into the zinc oxide. Not given: how much paste, or the strength of the epoxy solution.
གོམ་པ་འདིའི་རྫས་རིགས:
བིས་མུཏ་ཨོག་སཱའིཌ།1 as requiredལག་ཆས་དགོས་མཁོ:
ཨེ་པོག་སི་ཞུན་ཤིང
n-བུ་ཊ་ནོལ།
མཱཕལ་ཐབ5
5
Spray aluminium electrodes and attach leads
Spray aluminium electrodes and attach leads
Spray a metallised film of aluminium on both faces. Attach a lead wire to each with conductive silver paint, as in Example 1. Unknown: the spraying method and the paint.
གོམ་པ་འདིའི་རྫས་རིགས:
ཨེལུ་མི་ནི་ཡམ་གྱི་གོང་བུ།1 as required
དངུལ་གྱི་གློག་འཁྱོར་ཚོན1 as required
ཟངས་ཐག2 དུམ་བུ།ལག་ཆས་དགོས་མཁོ:
མ་ཤེས་པའི་ལྕགས་གཏོར་ཐབས།
བར་ནི་ཡར་གྱི་འཇལ་ཆས།རྫས་རིགས
5- 1 as requiredས་ཆ་འཛིན
- 1 as requiredས་ཆ་འཛིན
- 1 as requiredས་ཆ་འཛིན
- 1 as requiredས་ཆ་འཛིན
- 2 དུམ་བུ།ས་ཆ་འཛིན
ལག་ཆས་དགོས་མཁོ
9- ས་ཆ་འཛིན
- ས་ཆ་འཛིན
- ས་ཆ་འཛིན
- ས་ཆ་འཛིན
- ས་ཆ་འཛིན
- ས་ཆ་འཛིན
- ས་ཆ་འཛིན
- ས་ཆ་འཛིན
- ས་ཆ་འཛིན
བིལུ་པིརིན་ཊི་འདི་གིས་བཟོ་མི
འབྲེལ་ཡོད་བིལུ་པིརིན་ཊི
བིལུ་པིརིན་ཊི་འདི་ཚུ་ཐབས་ལམ་དང་རྫས་རིགས། སྤྱི་ཆོས་བགོ་བཤའ་བྱེད
CC0 སྤྱི་དབང
བིལུ་པིརིན་ཊི་འདི་CC0 འོག་བཀྲམས་ཡོད། ཁྱེད་རང་གིས་ཆོག་མཆན་མ་བཞེས་པར་ཕབ་ལེན་དང་བཟོ་བཅོས། བགོ་བཤའ། དགོས་མཁོ་གང་ལའང་བཀོལ་སྤྱོད་བྱས་ཆོག
བཟོ་མཁན་ལ་རྒྱབ་སྐྱོར་བྱེད་པའི་ཆེད་ཁོང་ཚོའི་བིལུ་པིརིན་ཊི་བརྒྱུད་ཐོན་སྐྱེད་ཉོ། བཟོ་མཁན་གྱིས བཟོ་མཁན་གྱི་ཁེ་ཕོགས ཚོང་པས་གཏན་འཁེལ་བྱས་པ། ཡང་ན་བིལུ་པིརིན་ཊི་འདིའི་པར་གསར་བཟོས་ཏེ་ཁྱེད་རང་གི་བིལུ་པིརིན་ཊི་ནང་མཐུད་སྦྲེལ་བྱས་ཏེ་ཡོང་སྒོ་བགོ་བཤའ་བྱེད།