Metal Oxide Varistor: Zinc Oxide with Manganese and Chromic Oxides, Bismuth Paste Fired On (Masuyama 1972, Ex. 6)
A varistor with manganese dioxide and chromic oxide mixed into the zinc oxide, and bismuth oxide fired on from a paste: 99.0 % zinc oxide, 0.5 % manganese dioxide and 0.5 % chromic oxide by moles, sintered at 1350 °C, coated with bismuth oxide paste and fired at 800 °C. The disc measured a C-value of 282 at 1 mA and a nonlinearity exponent n of 25.6.
Source: T. Masuyama, M. Matsuoka and T. Nishi (Matsushita), US 3,663,458 (1972), Example 6. Unknown: how the aluminium is sprayed on, what the silver paint is, and how strong the epoxy solution of the paste is. The 10 g batch is our arithmetic. Picture: the patent's drawing.
མཐོ་རིམ
2 days
ལམ་སྟོན
1
1
Weigh 99 : 0.5 : 0.5 and wet-mill 5 hours
Weigh 99 : 0.5 : 0.5 and wet-mill 5 hours
Mix zinc oxide, manganese dioxide and chromic oxide 99 : 0.5 : 0.5 by moles. Ours, for 10 g: 9.854 g zinc oxide, 0.053 g manganese dioxide, 0.093 g chromic oxide (our arithmetic). Mill wet for 5 hours, then dry, as in Example 1. Unknown: the milling liquid.
གོམ་པ་འདིའི་རྫས་རིགས:
ཟིངཀ་ཨོག་སའིཌ་ཕུད་རྡུལ9.854 g
མང་ག་ནིསི་ཌའི་ཨོག་སའིཌི། (པའི་རོ་ལུ་སའིཊི)0.053 g
ཀྲོ་མིཀ་ཨོཀ་སཱའིཌ།0.093 gལག་ཆས་དགོས་མཁོ:
ལག་པ་འདྲ་མཉམ་གྱི་སྲང་།
ལྕགས་ཀྱི་ལྡེ་གུ་འཚོག་འཁོར་ལོ
སྐམ་ནིའི་ཐབ2
2
Press discs 13 mm by 2.5 mm
Press discs 13 mm by 2.5 mm
Press discs 13 mm across and 2.5 mm thick at 340 kg/cm², as in Example 1.
ལག་ཆས་དགོས་མཁོ:
ཧའི་ཌོ་ལིཀ་ནོན་འཕྲུལ།
སྡེར་ཆས་ནན་བཙིར་གྱི་ དཔེ་ཚད།
བར་ནི་ཡར་གྱི་འཇལ་ཆས།3
3
Sinter 1 hour at 1350 °C and furnace-cool
Sinter 1 hour at 1350 °C and furnace-cool
Sinter in air at 1350 °C for 1 hour and let the discs cool in the furnace.
ལག་ཆས་དགོས་མཁོ:
མཱཕལ་ཐབ4
4
Lap both faces
Lap both faces
Lap both faces with silicon carbide abrasive. Example 6 gives no thickness.
ལག་ཆས་དགོས་མཁོ:
བར་ནི་ཡར་གྱི་འཇལ་ཆས།5
5
Coat with bismuth oxide paste and fire at 800 °C
Coat with bismuth oxide paste and fire at 800 °C
Coat both lapped faces with a paste of 50 % by weight bismuth oxide in a solution of epoxy resin in butyl alcohol, and fire it in air at 800 °C for 30 minutes. The bismuth oxide diffuses into the zinc oxide. Not given: how much paste, or the strength of the epoxy solution.
གོམ་པ་འདིའི་རྫས་རིགས:
བིས་མུཏ་ཨོག་སཱའིཌ།1 as requiredལག་ཆས་དགོས་མཁོ:
ཨེ་པོག་སི་ཞུན་ཤིང
n-བུ་ཊ་ནོལ།
མཱཕལ་ཐབ6
6
Spray aluminium electrodes and attach leads
Spray aluminium electrodes and attach leads
Spray a metallised film of aluminium on both faces. Attach a lead wire to each with conductive silver paint, as in Example 1. Unknown: the spraying method and the paint.
གོམ་པ་འདིའི་རྫས་རིགས:
ཨེལུ་མི་ནི་ཡམ་གྱི་གོང་བུ།1 as required
དངུལ་གྱི་གློག་འཁྱོར་ཚོན1 as required
ཟངས་ཐག2 དུམ་བུ།ལག་ཆས་དགོས་མཁོ:
མ་ཤེས་པའི་ལྕགས་གཏོར་ཐབས།
བར་ནི་ཡར་གྱི་འཇལ་ཆས།རྫས་རིགས
7- 9.854 gས་ཆ་འཛིན
- ས་ཆ་འཛིན
- 0.093 gས་ཆ་འཛིན
- 1 as requiredས་ཆ་འཛིན
- 1 as requiredས་ཆ་འཛིན
- 1 as requiredས་ཆ་འཛིན
- 2 དུམ་བུ།ས་ཆ་འཛིན
ལག་ཆས་དགོས་མཁོ
11- ས་ཆ་འཛིན
- ས་ཆ་འཛིན
- ས་ཆ་འཛིན
- ས་ཆ་འཛིན
- ས་ཆ་འཛིན
- ས་ཆ་འཛིན
- ས་ཆ་འཛིན
- ས་ཆ་འཛིན
- ས་ཆ་འཛིན
- ས་ཆ་འཛིན
- ས་ཆ་འཛིན
བིལུ་པིརིན་ཊི་འདི་གིས་བཟོ་མི
འབྲེལ་ཡོད་བིལུ་པིརིན་ཊི
བིལུ་པིརིན་ཊི་འདི་ཚུ་ཐབས་ལམ་དང་རྫས་རིགས། སྤྱི་ཆོས་བགོ་བཤའ་བྱེད
CC0 སྤྱི་དབང
བིལུ་པིརིན་ཊི་འདི་CC0 འོག་བཀྲམས་ཡོད། ཁྱེད་རང་གིས་ཆོག་མཆན་མ་བཞེས་པར་ཕབ་ལེན་དང་བཟོ་བཅོས། བགོ་བཤའ། དགོས་མཁོ་གང་ལའང་བཀོལ་སྤྱོད་བྱས་ཆོག
བཟོ་མཁན་ལ་རྒྱབ་སྐྱོར་བྱེད་པའི་ཆེད་ཁོང་ཚོའི་བིལུ་པིརིན་ཊི་བརྒྱུད་ཐོན་སྐྱེད་ཉོ། བཟོ་མཁན་གྱིས བཟོ་མཁན་གྱི་ཁེ་ཕོགས ཚོང་པས་གཏན་འཁེལ་བྱས་པ། ཡང་ན་བིལུ་པིརིན་ཊི་འདིའི་པར་གསར་བཟོས་ཏེ་ཁྱེད་རང་གི་བིལུ་པིརིན་ཊི་ནང་མཐུད་སྦྲེལ་བྱས་ཏེ་ཡོང་སྒོ་བགོ་བཤའ་བྱེད།