Barium Ferrite Disc Magnet: Barium Carbonate and Iron Oxide Sintered (Went, Philips 1956)
Charlie

创建者

Charlie

28. 十月 2026DE
2
0
0
0
0

Barium Ferrite Disc Magnet: Barium Carbonate and Iron Oxide Sintered (Went, Philips 1956)

The dark grey ceramic magnet on fridges and in loudspeakers is barium ferrite. It is made from two cheap powders: one part barium carbonate to six of iron oxide, milled, fired, milled again, pressed and sintered. No cobalt or nickel is needed. This is Example 34 of the Philips patent. Fired 4 hours at 1100 °C, its rod held 1,375 gauss with a coercive force of 3,350 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956). They pressed rods; the claim covers "a body of a desired shape", and the disc size is ours. The patent does not say how to magnetise it; our way is stated. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
高级
2 days

说明

1

Weigh one part barium carbonate to six of iron oxide

Weigh 39.5 g of barium carbonate (0.2 mol) and 191.7 g of ferric oxide, Fe2O3 (1.2 mol). Barium carbonate is poisonous if swallowed: ours, gloves and a dust respirator.

此步骤所需材料:

碳酸钡(毒重石)碳酸钡(毒重石)39.5 克
氧化铁氧化铁191.7 克

所需工具:

等臂天平等臂天平
橡胶手套橡胶手套
P100 防毒面具P100 防毒面具
2

Mill with ethanol for 4 hours

Grind the mixture with ethanol in an iron ball mill for 4 hours. Let the ethanol evaporate, then dry the powder in a drying oven.

所需工具:

铁球磨机铁球磨机
乙醇——实验级,95 %乙醇——实验级,95 %
干燥炉干燥炉
3

Presinter at 1000 °C for 4 hours

Fire the dry powder in air at 1000 °C for 4 hours (ours: in a lidded porcelain crucible in a muffle furnace). Let it cool.

所需工具:

马弗炉马弗炉
带盖坩埚(瓷质)带盖坩埚(瓷质)
坩埚钳坩埚钳
耐热手套耐热手套
4

Mill again for 4 hours

Grind the presintered product with ethanol in the ball mill for another 4 hours. Let the ethanol evaporate.

所需工具:

铁球磨机铁球磨机
乙醇——实验级,95 %乙醇——实验级,95 %
干燥炉干燥炉
P100 防毒面具P100 防毒面具
5

Press discs at 1.5 tons per cm²

Press the powder at 1.5 tons/cm². The patent pressed rods; we press discs. Ours: a die 20 mm across, so about 4.7 tonnes on the punch (our arithmetic: 1.5 × 3.14 cm²).

所需工具:

液压机液压机
圆片压模圆片压模
6

Sinter for 4 hours

Sinter the discs for 4 hours in oxygen or in air. The patent's results: at 1100 °C, 1,375 gauss and 3,350 oersted; at 1200 °C, 1,400 and 3,100; at 1300 °C, 1,850 and 1,780. Hotter gives a stronger but less stubborn magnet.

所需工具:

马弗炉马弗炉
坩埚钳坩埚钳
耐热手套耐热手套
7

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

所需工具:

电磁铁电磁铁
指南针指南针

材料

2

所需工具

14

CC0 公共领域

此蓝图以 CC0 协议发布。你可以自由复制、修改、分发和使用此作品,无需征得许可。

通过购买蓝图中的产品支持创客,他们将获得 创客佣金 (由供应商设定),或创建此蓝图的新版本并将其作为连接包含在你自己的蓝图中以分享收入。

讨论

(0)

登录 加入讨论

加载评论中...