Extruded Polystyrene Foam: Butylene-Blown Logs 20 Inches Across (McIntire, Dow 1948, Ex. 4)
Extruded polystyrene foam blown with a butylene gas fraction. 300 lb of polystyrene and about 130 lb of the fraction stand two days at 110 °C under 265 psi. Opened again and again, the tower let out foam logs 20 inches across and 20 feet long, weighing only 0.8 lb per cubic foot. Unknown: a source for the butylene fraction, linked to an unknown head.
Source: O. R. McIntire (Dow), US 2,450,436 (1948), Example 4. Picture: the patent's drawing.
高级
3 days
说明
1
1
Charge the tower with polystyrene
Charge the tower with polystyrene
Charge a high-pressure tower with 300 lb of granular polystyrene.
此步骤所需材料:
聚苯乙烯300 磅所需工具:
压力反应器
等臂天平
橡胶手套2
2
Add the butylene fraction
Add the butylene fraction
Add about 130 lb of a cracked-oil gas fraction that is about 87 % normal butylenes, with some butanes and butadiene, under pressure. Unknown: a source for this fraction. Flammable gas: no flames, strong ventilation.
此步骤所需材料:
丁烯裂解气馏分130 磅所需工具:
高压气瓶
压力反应器
化学防溅护目镜3
3
Heat two days at 110 °C
Heat two days at 110 °C
Close the tower and heat it at 110 °C for two days. The gauge pressure stays at 265 psi.
所需工具:
压力反应器
实验室温度计4
4
Let out logs through a 3.25 inch outlet
Let out logs through a 3.25 inch outlet
Open and close the 3.25 inch outlet near the bottom again and again. Each portion swells into a foam log 20 inches across and about 20 feet long, with fine, even, closed cells, weighing 0.8 lb per cubic foot.
所需工具:
压力反应器
化学防溅护目镜
橡胶手套5
5
Saw into boards
Saw into boards
When the foam has set, saw it lengthwise into slabs (ours: a woodworking saw).