Ferromolybdenum: Molybdic Oxide Smelted with Coke and Lime into Molten Steel in an Electric Arc Furnace (Brigham, US 4,160,661)

Technical molybdic oxide is fed in cans, with coke and lime, into a bath of molten steel in a 3000 kVA arc furnace. The electrodes stay in the slag, and the coke is trimmed after every charge unit so the metal keeps under 0.1 % carbon. Ferrosilicon and lime strip the slag, and the metal is shotted in running water. Result: from 5000 lb oxide, 3110 lb shot and pig of 54.1 % molybdenum, 0.06 % carbon, 43.1 % iron (Heat 4), using 1.94 kWh per lb of molybdenum. Source: Brigham, Sirianni and Garner, US patent 4,160,661 (1979), Example 2, Heat 4. Not given: how the shot was heated while drying overnight. Picture drawn by Youblob.
高级
1 day

说明

1

Melt the steel

In a three-phase 3000 kVA arc furnace with 8 in graphite electrodes, lined with magnesia brick and rammed basic refractory (about 60 % MgO), 5 ft 6 in across and 26 in deep below the tap hole, melt 812 lb steel plate with 80 lb burnt lime under full power. Lead the fume to a bag house.

此步骤所需材料:

低碳钢板低碳钢板812 磅

所需工具:

生石灰生石灰
电弧炉电弧炉
石墨电极石墨电极
布袋除尘室布袋除尘室
2

Make up the charge units

While it melts, weigh out five charge units, each 1000 lb molybdic oxide (in cans of 37 lb oxide in a 2 lb steel can), 250 lb coke and 320 lb lime. For Heat 4 that was 5000 lb oxide, 1150 lb coke, 1600 lb lime and 1488 lb steel in plate and cans. Ours: metallurgical coke for the dried breeze coke.

此步骤所需材料:

工业氧化钼工业氧化钼5000 磅
低碳钢板低碳钢板1488 磅

所需工具:

冶金焦炭冶金焦炭
生石灰生石灰
工业平台秤工业平台秤
3

Smelt in the bath

When the bath is molten at about 1450 °C, add one can of oxide with equal shovels of coke and lime every 2 minutes, about 1 hour per unit. Use the 205 V tap so the electrodes dip only into the slag; hold the bath at most 1760 °C. About 1 kWh per lb of oxide.

所需工具:

铁锹铁锹
电弧炉电弧炉
4

Keep the carbon down

After every charge unit, dip a steel spoon into the bath and analyse the carbon (about 15 minutes); cut the coke so the metal stays below 0.1 % carbon.

所需工具:

冶金焦炭冶金焦炭
5

Strip the slag and tap

Add 200 lb ferrosilicon and 560 lb lime to strip the slag. Tip the furnace into a preheated 5000 lb ladle: the first ladle is mostly slag, the second mostly metal. Back-pour the slag into slag pots.

所需工具:

硅铁硅铁
生石灰生石灰
铸造浇包铸造浇包
6

Shot the metal

Pour the metal from the ladle into a second unlined 5000 lb ladle filled with running water from a 2 1/4 in fire hose, about 3000 lb a minute, from about 4 ft up; 2000 lb shots in 10 to 15 minutes. Dry the shot overnight at about 300 °F in 40 gallon drums. Ours: a drying oven.

所需工具:

铸造浇包铸造浇包
水水
干燥炉干燥炉

材料

2

所需工具

11

此蓝图制作

CC0 公共领域

此蓝图以 CC0 协议发布。你可以自由复制、修改、分发和使用此作品,无需征得许可。

通过购买蓝图中的产品支持创客,他们将获得 创客佣金 (由供应商设定),或创建此蓝图的新版本并将其作为连接包含在你自己的蓝图中以分享收入。

讨论

(0)

登录 加入讨论

加载评论中...