A paint for putting silver electrodes on ceramic, glass or mica. Silver oxide and a little ceramic flux are held in polyvinyl alcohol dissolved in water. The wet paint conducts electricity, so a capacitor can be measured while it is being painted. On firing, the silver oxide turns into a silver film held on by the flux. Gray found this paint so stable that it kept six months.
Source: Robert B. Gray, US 2,695,275 (Erie Resistor, 1954), Example 2. Not given: which flux, and the firing heat. Bismuth subnitrate, one of the fluxes Gray names, is ours. Picture drawn by Youblob.
初学者
1 day
说明
1
1
Dissolve 2 g polyvinyl alcohol in the water
Dissolve 2 g polyvinyl alcohol in the water
For 100 g of paint: dissolve 2 g polyvinyl alcohol in the water, warming it to help it dissolve. The water is the balance, about 34 to 44 g. Warming is ours.
此步骤所需材料:
聚乙烯醇粉末2 克
蒸馏水1 as required所需工具:
等臂天平
硼硅玻璃烧杯
电热板
硼硅玻璃棒2
2
Grind in silver oxide and flux
Grind in silver oxide and flux
Grind 50 g precipitated silver oxide and 2 to 10 g ceramic flux into the solution until smooth. Gray gives the flux only as a class; ours: bismuth subnitrate, one of the common fluxes he names. The right amount depends on the ceramic it will be fired onto.
此步骤所需材料:
氧化银50 克
次硝酸铋1 as required所需工具:
等臂天平
研钵与研杵
丁腈手套3
3
Add 2 to 4 g alcohol against foam
Add 2 to 4 g alcohol against foam
Stir in 2 to 4 g ethyl alcohol. It stops the polyvinyl alcohol from foaming.
此步骤所需材料:
乙醇——实验级,95 %1 as required所需工具:
硼硅玻璃棒4
4
Store
Store
Keep it in a closed jar. Gray found no reaction between the ingredients in six months, and the paint can stand for some hours in use without stirring.
所需工具:
深色玻璃密封罐材料
5- 2 克占位符
- 1 as required占位符
- 50 克占位符
- 1 as required占位符
- 1 as required占位符
此蓝图制作
相关蓝图
这些蓝图共享知识——技术、材料或原理
CC0 公共领域
此蓝图以 CC0 协议发布。你可以自由复制、修改、分发和使用此作品,无需征得许可。
通过购买蓝图中的产品支持创客,他们将获得 创客佣金 (由供应商设定),或创建此蓝图的新版本并将其作为连接包含在你自己的蓝图中以分享收入。