Phosphor Bronze Ingot: 90 Copper Melted under Charcoal with 10 Phosphor-Tin, Stirred with Graphite (Thurston)
Phosphor bronze is a tin bronze cleaned of oxide by a little phosphorus, which makes it sound, tough and springy. Thurston melts the copper under charcoal, stirs in phosphor-tin with a graphite bar, skims and pours at once.
Result: phosphor bronze of 90 parts copper and 10 parts phosphor-tin, cast into ingots.
Source: Thurston, A Treatise on Brasses, Bronzes and Other Alloys (1910), pp. 145-147. Not given: temperatures, mould. Picture drawn by Youblob.
中级
1 day
说明
1
1
Weigh 90 copper to 10 phosphor-tin
Weigh 90 copper to 10 phosphor-tin
Weigh 90 parts of copper to 10 parts of phosphor-tin, Thurston's mix for coupling and crank-rod journals. Use no zinc.
此步骤所需材料:
铜锭90 parts by weight
磷锡10 parts by weight所需工具:
等臂天平2
2
Melt the copper under charcoal
Melt the copper under charcoal
Melt the copper in a plumbago crucible and cover it with charcoal as quickly as possible.
所需工具:
石墨黏土坩埚
坩埚炉
木炭3
3
Stir in the phosphor-tin with a graphite bar
Stir in the phosphor-tin with a graphite bar
Add the phosphor-tin while stirring the metal continually and carefully with a graphite bar, a strip of old plumbago crucible or a bar of retort carbon.
所需工具:
石墨电极4
4
Skim and pour before a skin forms
Skim and pour before a skin forms
Clear the charcoal and dross off the top and pour before the surface begins to skin over. If the metal does not show a bright mirror face, a tiny further addition of phosphor metal is needed.
所需工具:
漏勺
坩埚钳
锭模此蓝图制作