艺术
美容与健康
工艺
文化与历史
娱乐
环境
食品与饮料
逆向工程
科学
体育
技术
可穿戴设备
Semi-Cured Phenolic Sheet: Paper Dipped in Phenol Resin and Part-Cured at 120-130 °C (Lucas, Western Electric, US 1,470,990)
Charlie

创建者

Charlie

31. 十月 2026DE
1
0
0
0
0

Semi-Cured Phenolic Sheet: Paper Dipped in Phenol Resin and Part-Cured at 120-130 °C (Lucas, Western Electric, US 1,470,990)

Paper soaked in phenol resin is dried, then cured only part of the way, so the resin is stiff but not yet hard. Lucas did this before the final hot press so the press would not squeeze the resin out of the fibres. Result: a dry, partly cured phenolic sheet that a later coat of phenolic resin can still bond into. Source: Lucas, US 1,470,990 (Western Electric, 1923). Stopping before his final hot press is ours. Not given: the solvent in his resin, paper grade, mercerising strengths. Picture drawn by Youblob.
中级
1 hour

说明

1

Dip the paper in phenol resin

Run the paper through a bath of phenol resin of specific gravity about 0.970: about 2 minutes for plain paper, 1 minute or less if mercerised first. Ours: Liquid Bakelite as the resin; Lucas does not say how it was thinned.

此步骤所需材料:

纸纸1 as required
液态酚醛树脂(苯酚-甲醛缩合产物)液态酚醛树脂(苯酚-甲醛缩合产物)1 as required

所需工具:

半固化片浸渍生产线半固化片浸渍生产线
比重计比重计
2

Optional: mercerise the paper first

For faster, fuller soaking, first pass the paper through caustic soda, squeeze, wash in water, neutralise in an acid, wash again and dry. Strengths and the acid: not given.

所需工具:

烧碱(氢氧化钠)烧碱(氢氧化钠)
半固化片浸渍生产线半固化片浸渍生产线
3

Dry at about 90 °C

Dry the soaked paper in an oven at about 90 °C, just long enough to dry it.

所需工具:

干燥炉干燥炉
4

Part-cure at 120-130 °C

Pass the dry paper through a curing oven at 120-130 °C for about 10 minutes (Lucas's description; his claim 4 says 125 °C for about 10 seconds). The resin sets as stiff as the fibres, but does not harden through.

所需工具:

固化烘箱固化烘箱
5

Dip again for 10-15 seconds and dry

Dip the part-cured paper in phenol resin again for 10-15 seconds, then dry at about 90 °C until it can be wound on a reel. Stop here: the sheet is semi-cured. Lucas's next step, stacking and hot pressing, cures it fully.

此步骤所需材料:

液态酚醛树脂(苯酚-甲醛缩合产物)液态酚醛树脂(苯酚-甲醛缩合产物)1 as required

所需工具:

半固化片浸渍生产线半固化片浸渍生产线
干燥炉干燥炉

材料

2

所需工具

5

CC0 公共领域

此蓝图以 CC0 协议发布。你可以自由复制、修改、分发和使用此作品,无需征得许可。

通过购买蓝图中的产品支持创客,他们将获得 创客佣金 (由供应商设定),或创建此蓝图的新版本并将其作为连接包含在你自己的蓝图中以分享收入。