Silicone Rubber Compound: Dimethyl Silicone Oil Gelled with Ferric Oxide, Agens 1948
Dimethyl silicone oil mixed with three-quarters its weight of red ferric oxide and a little aluminium chloride, heated to 130 °C, thins and then sets to a solid mass; milled on warm rubber rolls it becomes a silicone rubber compound ready to mould or extrude (Agens, General Electric, US 2,448,756, 1948). Cured, it stretches over 100 % and stays flexible at −60 °C.
The picture: our drawing of the beaker, the mill and the sheet.
高级
A day
说明
1
1
Weigh the mix
Weigh the mix
To 400 g silicone oil add 300 g ferric oxide (75 % of the oil) and 5 g anhydrous aluminium chloride (1.25 %). Stir it smooth. Keep the chloride dry; it fumes in damp air.
此步骤所需材料:
细红抛光粉300 克所需工具:
氯化铝(无水)
硼硅玻璃烧杯
搅拌器
数字厨房秤
橡胶手套2
2
Heat to 130 °C
Heat to 130 °C
Heat the mix to 130 °C. It first gets thinner, then thickens fast until the whole mass is solid.
所需工具:
电热板
温度计
硼硅玻璃烧杯3
3
Mill and sheet
Mill and sheet
Work the mass on rubber rolls at 125 °C for about half an hour and take it off as a sheet. This is the compound.
所需工具:
双辊开炼机
温度计4
4
Test a piece
Test a piece
Agens's test: press a sheet about 1.3 mm thick between platens at 150 °C for ten minutes, then 15 minutes in an oven at 200 °C. It should stretch over twice its length.
所需工具:
加热模压机
退火炉5
5
The mix
The mix
正在加载 Jupyter 笔记本…
此蓝图制作
相关蓝图
这些蓝图共享知识——技术、材料或原理
CC0 公共领域
此蓝图以 CC0 协议发布。你可以自由复制、修改、分发和使用此作品,无需征得许可。
通过购买蓝图中的产品支持创客,他们将获得 创客佣金 (由供应商设定),或创建此蓝图的新版本并将其作为连接包含在你自己的蓝图中以分享收入。