Ytterbium: Oxide Reduced by Lanthanum at 1020 °C in Vacuum, Metal Distilled Off (Shindo and Yagi, US 2010/0260640)
Charlie

创建者

Charlie

1. 十一月 2026DE
5
0
0
0
0

Ytterbium: Oxide Reduced by Lanthanum at 1020 °C in Vacuum, Metal Distilled Off (Shindo and Yagi, US 2010/0260640)

Ytterbium boils far more easily than lanthanum. Heated with lanthanum in a vacuum, ytterbium oxide gives up its oxygen to the lanthanum, and the freed ytterbium leaves as vapour and condenses in a cooler zone, while lanthanum oxide stays behind. Result: ytterbium metal ingots; 20 kg of distillate in the patent's run, low in sodium, potassium and lithium. Source: Y. Shindo and K. Yagi, US patent application 2010/0260640 (2010), Example 1. Not given: how much lanthanum, the vacuum, the time, crucible and condenser materials. Picture drawn by Youblob.
高级
1 day

说明

1

Mix the oxide with lanthanum

Mix ytterbium oxide with lanthanum metal as the reducing agent. Not given: the proportions.

此步骤所需材料:

氧化镱氧化镱1 as required

所需工具:

镧镧
钽坩埚钽坩埚
2

Reduce in vacuum at 1020 °C

Heat the charge in a vacuum to 1020 °C: Yb2O3 + 2 La -> 2 Yb (vapour) + La2O3. Ours: a vacuum induction furnace; the vacuum level and time are not given.

所需工具:

感应炉感应炉
真空泵真空泵
钽坩埚钽坩埚
3

Condense the ytterbium at 200-600 °C

Catch the ytterbium vapour on a condenser held at 200-600 °C. Most of it settles in the 300-500 °C part; the 200-300 °C part carries the least sodium and lithium. Ours: a tantalum condenser plate.

所需工具:

钽冷凝板钽冷凝板
4

Melt into ingots under argon

Take the distillate off the condenser, melt it in a crucible at 950 °C under a slight pressure of argon, and let it solidify into an ingot.

所需工具:

钽坩埚钽坩埚
感应炉感应炉
氩氩

材料

1
  • 1 as required
    占位符

所需工具

6
  • 占位符
  • 占位符
  • 占位符
  • 1 vendor sell this, none ship to you yet