Metal Oxide Varistor: Zinc Oxide with 0.5 % Antimony Trioxide, Bismuth Oxide Paste Fired On (Masuyama 1972, Ex. 5)
A varistor with bismuth oxide fired on from a paste instead of mixed in: 99.5 % zinc oxide with 0.5 % antimony trioxide by moles, sintered at 1350 °C, coated with bismuth oxide paste and fired at 800 °C. The disc measured a C-value of 130 at 1 mA and a nonlinearity exponent n of 19.7.
Source: T. Masuyama, M. Matsuoka and T. Nishi (Matsushita), US 3,663,458 (1972), Example 5. Unknown: how the aluminium is sprayed on, what the silver paint is, and how strong the epoxy solution of the paste is. The 10 g batch is our arithmetic. Picture: the patent's drawing.
高级
2 days
说明
1
1
Weigh 99.5 : 0.5 and wet-mill 5 hours
Weigh 99.5 : 0.5 and wet-mill 5 hours
Mix zinc oxide and antimony trioxide 99.5 : 0.5 by moles. Ours, for 10 g: 9.823 g zinc oxide and 0.177 g antimony trioxide (our arithmetic). Mill wet for 5 hours, then dry, as in Example 1. Unknown: the milling liquid.
此步骤所需材料:
氧化锌粉末9.823 克
三氧化二锑0.177 克所需工具:
等臂天平
铁球磨机
干燥炉2
2
Press discs 13 mm by 2.5 mm
Press discs 13 mm by 2.5 mm
Press discs 13 mm across and 2.5 mm thick at 340 kg/cm², as in Example 1.
所需工具:
液压机
圆片压模
游标卡尺3
3
Sinter 1 hour at 1350 °C and furnace-cool
Sinter 1 hour at 1350 °C and furnace-cool
As in Example 2: sinter in air at 1350 °C for 1 hour and let the discs cool in the furnace.
所需工具:
马弗炉4
4
Lap both faces
Lap both faces
Lap both faces with silicon carbide abrasive. Example 5 gives no thickness.
所需工具:
游标卡尺5
5
Coat with bismuth oxide paste and fire at 800 °C
Coat with bismuth oxide paste and fire at 800 °C
Coat both lapped faces with a paste of 50 % by weight bismuth oxide in a solution of epoxy resin in butyl alcohol, and fire it in air at 800 °C for 30 minutes. The bismuth oxide diffuses into the zinc oxide. Not given: how much paste, or the strength of the epoxy solution.
此步骤所需材料:
氧化铋1 as required所需工具:
环氧树脂
正丁醇
马弗炉6
6
Spray aluminium electrodes and attach leads
Spray aluminium electrodes and attach leads
Spray a metallised film of aluminium on both faces. Attach a lead wire to each with conductive silver paint, as in Example 1. Unknown: the spraying method and the paint.
此步骤所需材料:
铝锭1 as required
银导电漆1 as required
铜线2 个所需工具:
未知的金属喷涂方法
游标卡尺材料
6- 9.823 克占位符
- 0.177 克占位符
- 1 as required占位符
- 1 as required占位符
- 1 as required占位符
- 2 个占位符
相关蓝图
这些蓝图共享知识——技术、材料或原理
CC0 公共领域
此蓝图以 CC0 协议发布。你可以自由复制、修改、分发和使用此作品,无需征得许可。
通过购买蓝图中的产品支持创客,他们将获得 创客佣金 (由供应商设定),或创建此蓝图的新版本并将其作为连接包含在你自己的蓝图中以分享收入。