Metal Oxide Varistor: Zinc Oxide with Manganese and Titanium Oxides, Bismuth Paste Fired On (Masuyama 1972, Ex. 6)
Ed

创建者

Ed

28. 十月 2026FI
4
0
0
0
0

Metal Oxide Varistor: Zinc Oxide with Manganese and Titanium Oxides, Bismuth Paste Fired On (Masuyama 1972, Ex. 6)

A varistor with manganese dioxide and titanium dioxide mixed into the zinc oxide, and bismuth oxide fired on from a paste: 99.0 % zinc oxide, 0.5 % manganese dioxide and 0.5 % titanium dioxide by moles, sintered at 1350 °C, coated with bismuth oxide paste and fired at 800 °C. The disc measured a C-value of 66 at 1 mA and a nonlinearity exponent n of 13.7. Source: T. Masuyama, M. Matsuoka and T. Nishi (Matsushita), US 3,663,458 (1972), Example 6. Unknown: how the aluminium is sprayed on, what the silver paint is, and how strong the epoxy solution of the paste is. The 10 g batch is our arithmetic. Picture: the patent's drawing.
高级
2 days

说明

1

Weigh 99 : 0.5 : 0.5 and wet-mill 5 hours

Mix zinc oxide, manganese dioxide and titanium dioxide 99 : 0.5 : 0.5 by moles. Ours, for 10 g: 9.898 g zinc oxide, 0.053 g manganese dioxide, 0.049 g titanium dioxide (our arithmetic). Mill wet for 5 hours, then dry, as in Example 1. Unknown: the milling liquid.

此步骤所需材料:

氧化锌粉末氧化锌粉末9.898 克
二氧化锰(软锰矿)二氧化锰(软锰矿)0.053 克
二氧化钛二氧化钛0.049 克

所需工具:

等臂天平等臂天平
铁球磨机铁球磨机
干燥炉干燥炉
2

Press discs 13 mm by 2.5 mm

Press discs 13 mm across and 2.5 mm thick at 340 kg/cm², as in Example 1.

所需工具:

液压机液压机
圆片压模圆片压模
游标卡尺游标卡尺
3

Sinter 1 hour at 1350 °C and furnace-cool

Sinter in air at 1350 °C for 1 hour and let the discs cool in the furnace.

所需工具:

马弗炉马弗炉
4

Lap both faces

Lap both faces with silicon carbide abrasive. Example 6 gives no thickness.

所需工具:

碳化硅磨料碳化硅磨料
游标卡尺游标卡尺
5

Coat with bismuth oxide paste and fire at 800 °C

Coat both lapped faces with a paste of 50 % by weight bismuth oxide in a solution of epoxy resin in butyl alcohol, and fire it in air at 800 °C for 30 minutes. The bismuth oxide diffuses into the zinc oxide. Not given: how much paste, or the strength of the epoxy solution.

此步骤所需材料:

氧化铋氧化铋1 as required

所需工具:

环氧树脂环氧树脂
正丁醇正丁醇
马弗炉马弗炉
6

Spray aluminium electrodes and attach leads

Spray a metallised film of aluminium on both faces. Attach a lead wire to each with conductive silver paint, as in Example 1. Unknown: the spraying method and the paint.

此步骤所需材料:

铝锭铝锭1 as required
银导电漆银导电漆1 as required
铜线铜线2 个

所需工具:

未知的金属喷涂方法未知的金属喷涂方法
游标卡尺游标卡尺

材料

7

所需工具

11

CC0 公共领域

此蓝图以 CC0 协议发布。你可以自由复制、修改、分发和使用此作品,无需征得许可。

通过购买蓝图中的产品支持创客,他们将获得 创客佣金 (由供应商设定),或创建此蓝图的新版本并将其作为连接包含在你自己的蓝图中以分享收入。

讨论

(0)

登录 加入讨论

加载评论中...