Acrylic Mirror Sheet: Silver Sprayed on Acrylic Treated with Tannin in Water and Acetic acid
Philips' Ponjee and Verwijlen (US 4,639,382, 1987) made silver hold on acrylic by first dipping it in tannin dissolved in water mixed with an organic solvent; tannin in plain water gave no bond. This is their acetic acid solution: 55–90 % water, 19–45 % acetic acid by volume, 3.3–5.5 g tannin per litre, which gave full bonding in their cross-cut test. The sheet is then sensitised with weak stannous chloride and silvered by spraying the silver solution and the reducer together.
The picture: our diagram.
Fortgeschritten
2 hours
Anweisungen
1
1
Dip in tannin solution for one minute
Dip in tannin solution for one minute
Make a solution of 3.3–5.5 g of tannic acid per litre in 55–90 % water and 19–45 % acetic acid by volume. Dip the acrylic sheet in it for one minute.
Materialien für diesen Schritt:
Acrylplatte1 StückBenötigte Werkzeuge:
Gerbsäure
Essigsäure (Eisessig)
Destilliertes Wasser
Glastabletts
Messzylinder
Balkenwaage
Abzug (mit Abluftanschluss)
Gummihandschuhe2
2
Rinse with water
Rinse with water
Rinse the sheet with water.
Benötigte Werkzeuge:
Destilliertes Wasser
Laborspritzflasche3
3
Spray with stannous chloride for 12 seconds
Spray with stannous chloride for 12 seconds
Spray the face to be silvered with a solution of 0.1 g stannous chloride and 0.1 ml concentrated hydrochloric acid per litre of water, for 12 seconds. Rinse off the excess with water.
Benötigte Werkzeuge:
Zinn(II)-chlorid
Salzsäure
Destilliertes Wasser
Wassersprühflasche
Laborspritzflasche
Chemikalienschutzbrille
Gummihandschuhe4
4
Spray silver and reducer together
Spray silver and reducer together
Atomise two solutions onto the face at the same time: silver nitrate with ammonia in water, and formalin in water. The patent gives no strengths: as required. Ours: a twin-nozzle spray gun.
Materialien für diesen Schritt:
Silbernitrat1 as requiredBenötigte Werkzeuge:
Ammoniaklösung 25-28 %
Formaldehydlösung (37 % Formalin)
Destilliertes Wasser
Doppeldüsen-Spritzpistole
Abzug (mit Abluftanschluss)
Chemikalienschutzbrille
GummihandschuheMaterialien
2- 1 StückPlatzhalter
- 1 as requiredPlatzhalter
Benötigte Werkzeuge
16- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
Dieser Bauplan stellt her
Verwandte Blueprints
Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien
CC0 Gemeinfrei
Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.
Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.