Acrylic Pellets: Methyl Methacrylate Stirred into Beads in Gelatine Water at 75 °C (Crawford & McGrath, ICI, US 2,108,044)
Stirred hard enough in water with a little gelatine, methyl methacrylate breaks into droplets that harden into separate beads of acrylic instead of one solid lump. ICI's beads settle out, wash easily and go straight to the moulding press.
Result: hard acrylic granules, used as moulding and extrusion pellets (they are beads, not cut pellets).
Source: Crawford & McGrath, US 2,108,044 (ICI, 1938), Examples 5 and 6. Picture drawn by Youblob.
Erfahren
1 day
Anweisungen
1
1
Dissolve 1 part benzoyl peroxide in 100 parts monomer
Dissolve 1 part benzoyl peroxide in 100 parts monomer
Dissolve 1 part by weight of benzoyl peroxide in 100 parts of methyl methacrylate.
Materialien für diesen Schritt:
Methylmethacrylat100 parts by weight
Benzoylperoxid1 part by weightBenötigte Werkzeuge:
Balkenwaage2
2
Mix with 200 parts of water holding 2 parts gelatine
Mix with 200 parts of water holding 2 parts gelatine
Mix it with 200 parts of water containing 2 parts of gelatine in solution (Example 6; Example 5 uses a soluble starch instead).
Benötigte Werkzeuge:
Gelatinepulver
Wasser
Polymerisationsreaktor mit Doppelmantel3
3
Stir at 1000 rpm and blow in steam to 75 °C
Stir at 1000 rpm and blow in steam to 75 °C
Stir at 1000 rpm and blow steam into the stirred mixture to bring it to 75 °C, and hold it there. After about 115 minutes the temperature starts to rise by itself: shut off the steam.
Benötigte Werkzeuge:
Rührer
Dampfkessel
Laborthermometer4
4
At the 82 °C peak, cool to 60 °C with cold water
At the 82 °C peak, cool to 60 °C with cold water
When the temperature peaks at 82 °C, cool the mixture to 60 °C by adding cold water.
Benötigte Werkzeuge:
Wasser5
5
Centrifuge, wash and dry at 100 °C
Centrifuge, wash and dry at 100 °C
Separate the granules in a centrifuge and wash them with 1 % hydrochloric acid, water, 2 % ammonia solution, and repeatedly with water. Dry them at 100 °C.
Benötigte Werkzeuge:
Korbzentrifuge
Salzsäure
Ammoniaklösung, verdünnt
TrockenofenMaterialien
2- 100 parts by weightPlatzhalter
- 1 part by weightPlatzhalter
Benötigte Werkzeuge
11- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
Dieser Bauplan stellt her
Verwandte Blueprints
Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien
CC0 Gemeinfrei
Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.
Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.