Barium-Calcium Ferrite Disc Magnet: 5 % Calcium, Sintered at 1330 °C (Went, Philips 1956, Ex. 18)

A ceramic magnet with a twentieth of the barium replaced by calcium: 0.095 mol barium carbonate, 0.005 mol calcium carbonate and 0.6 mol iron oxide. It is milled, fired in air, milled again, pressed and passed through a 1330 °C furnace in 10 minutes. The X-ray picture showed only the magnetoplumbite phase. Went's rod held 1,680 gauss with a coercive force of 1,110 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 18. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Erfahren
2 days

Anweisungen

1

Weigh barium carbonate, chalk and iron oxide

Weigh 18.74 g barium carbonate (0.095 mol), 0.5 g calcium carbonate (0.005 mol) and 95.55 g ferric oxide (0.6 mol). The patent used analytical-grade carbonates. Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Materialien für diesen Schritt:

Bariumcarbonat (Witherit)Bariumcarbonat (Witherit)18.74 g
Calciumcarbonat (Schlämmkreide)Calciumcarbonat (Schlämmkreide)0.5 g
Eisen(III)-oxidEisen(III)-oxid95.55 g

Benötigte Werkzeuge:

BalkenwaageBalkenwaage
GummihandschuheGummihandschuhe
P100-AtemschutzmaskeP100-Atemschutzmaske
2

Mill 4 hours, dry at 150 °C

Grind with alcohol in a ball mill for 4 hours and dry in air at 150 °C.

Benötigte Werkzeuge:

EisenkugelmühleEisenkugelmühle
Ethanol in Laborqualität, 95 %Ethanol in Laborqualität, 95 %
TrockenofenTrockenofen
3

Presinter in air at 1000 °C for 2 hours

Fire the dry powder in air at 1000 °C for 2 hours.

Benötigte Werkzeuge:

MuffelofenMuffelofen
Tiegel mit Deckel (Porzellan)Tiegel mit Deckel (Porzellan)
TiegelzangeTiegelzange
Hitzebeständige HandschuheHitzebeständige Handschuhe
4

Mill again, dry, press at 1.5 t/cm²

Grind again with alcohol for 4 hours, dry, and press at 1.5 tonnes per cm² (ours: discs instead of rods).

Benötigte Werkzeuge:

EisenkugelmühleEisenkugelmühle
Ethanol in Laborqualität, 95 %Ethanol in Laborqualität, 95 %
TrockenofenTrockenofen
Hydraulische PresseHydraulische Presse
Scheiben-PressformScheiben-Pressform
5

Pass through a 1330 °C zone in 10 minutes

Sinter at 1330 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

Benötigte Werkzeuge:

RohrofenRohrofen
Hitzebeständige HandschuheHitzebeständige Handschuhe
6

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Benötigte Werkzeuge:

ElektromagnetElektromagnet
KompassKompass

Materialien

3

Benötigte Werkzeuge

15

Dieser Bauplan stellt her

Verwandte Blueprints

Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...