Barium-Calcium Ferrite Disc Magnet: 0.09 mol BaCO3 and 0.01 mol CaCO3 (Went, Philips 1956, Ex. 19)
Charlie

Erstellt von

Charlie

28. Oktober 2026DE
6
0
0
0
0

Barium-Calcium Ferrite Disc Magnet: 0.09 mol BaCO3 and 0.01 mol CaCO3 (Went, Philips 1956, Ex. 19)

A ceramic magnet with a tenth of the barium replaced by calcium: 0.09 mol barium carbonate and 0.01 mol calcium carbonate to 0.6 mol iron oxide, made as in Example 18: milled, presintered at 1000 °C, milled again, formed and passed through a 1330 °C furnace in 10 minutes. Went's rod held 1,705 gauss with a coercive force of 1,110 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 19. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Erfahren
2 days

Anweisungen

1

Weigh barium carbonate, chalk and iron oxide

Weigh 17.76 g barium carbonate (0.09 mol), 1.001 g calcium carbonate (0.01 mol) and 95.55 g ferric oxide (0.6 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Materialien für diesen Schritt:

Bariumcarbonat (Witherit)Bariumcarbonat (Witherit)17.76 g
Calciumcarbonat (Schlämmkreide)Calciumcarbonat (Schlämmkreide)1.001 g
Eisen(III)-oxidEisen(III)-oxid95.55 g

Benötigte Werkzeuge:

BalkenwaageBalkenwaage
GummihandschuheGummihandschuhe
P100-AtemschutzmaskeP100-Atemschutzmaske
2

Mill with alcohol 4 hours, dry at 150 °C

Grind with alcohol in a ball mill for 4 hours and dry in air at 150 °C.

Benötigte Werkzeuge:

EisenkugelmühleEisenkugelmühle
Ethanol in Laborqualität, 95 %Ethanol in Laborqualität, 95 %
TrockenofenTrockenofen
3

Presinter in air at 1000 °C for 2 hours

Fire in air at 1000 °C for 2 hours.

Benötigte Werkzeuge:

MuffelofenMuffelofen
Tiegel mit Deckel (Porzellan)Tiegel mit Deckel (Porzellan)
TiegelzangeTiegelzange
Hitzebeständige HandschuheHitzebeständige Handschuhe
4

Mill again 4 hours, dry, form

Grind again with alcohol for 4 hours and dry. Example 19 extrudes a rod; ours: press discs at 1.5 tonnes per cm², as Example 18 moulds its rod.

Benötigte Werkzeuge:

EisenkugelmühleEisenkugelmühle
Ethanol in Laborqualität, 95 %Ethanol in Laborqualität, 95 %
TrockenofenTrockenofen
Hydraulische PresseHydraulische Presse
Scheiben-PressformScheiben-Pressform
5

Pass through a 1330 °C zone in 10 minutes

Sinter at 1330 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

Benötigte Werkzeuge:

RohrofenRohrofen
Hitzebeständige HandschuheHitzebeständige Handschuhe
6

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Benötigte Werkzeuge:

ElektromagnetElektromagnet
KompassKompass

Materialien

3

Benötigte Werkzeuge

15

Dieser Bauplan stellt her

Verwandte Blueprints

Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...