Barium Ferrite Disc Magnet: Fired in Carbon Dioxide, Pressed at 12 t/cm² (Went, Philips 1956, Ex. 33)

A barium ferrite made with more iron oxide, 0.4 mol barium carbonate to 3.6 mol, fired an hour at 1300 °C in carbon dioxide. Little oxygen gives the hexagonal crystal BaFe18O27, with some iron in the lower state. It is milled again, bound with nitrocellulose or polyvinyl alcohol, and pressed hard at 12 tonnes per cm². Went's rod held 1,260 gauss with a coercive force of 700 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 33. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Erfahren
2 days

Anweisungen

1

Weigh barium carbonate and iron oxide

Weigh 79.4 g barium carbonate (0.4 mol) and 580.9 g ferric oxide (3.6 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Materialien für diesen Schritt:

Bariumcarbonat (Witherit)Bariumcarbonat (Witherit)79.4 g
Eisen(III)-oxidEisen(III)-oxid580.9 g

Benötigte Werkzeuge:

BalkenwaageBalkenwaage
GummihandschuheGummihandschuhe
P100-AtemschutzmaskeP100-Atemschutzmaske
2

Mill 15.5 hours, press a pastille, fire in CO2

Grind with alcohol in a ball mill for 15.5 hours, dry, and press into a pastille. Heat it at 1300 °C in carbon dioxide for 1 hour (ours: a tube furnace fed from a CO2 cylinder).

Benötigte Werkzeuge:

EisenkugelmühleEisenkugelmühle
Ethanol in Laborqualität, 95 %Ethanol in Laborqualität, 95 %
TrockenofenTrockenofen
Hydraulische PresseHydraulische Presse
Scheiben-PressformScheiben-Pressform
RohrofenRohrofen
KohlendioxidgasKohlendioxidgas
DruckgasflascheDruckgasflasche
Hitzebeständige HandschuheHitzebeständige Handschuhe
3

Pulverise, mill 14 hours, bind

Crush the cooled pastille and grind it with alcohol for 14 hours. Press the powder into a pastille again with a ceramic binder (ours: polyvinyl alcohol, one of the two named), then crush it to grains.

Materialien für diesen Schritt:

Polyvinylalkohol-PulverPolyvinylalkohol-Pulver1 as required

Benötigte Werkzeuge:

EisenkugelmühleEisenkugelmühle
Ethanol in Laborqualität, 95 %Ethanol in Laborqualität, 95 %
Hydraulische PresseHydraulische Presse
Scheiben-PressformScheiben-Pressform
4

Press at 12 tonnes per cm²

Press the grains at 12 tonnes per cm² (ours: discs instead of rods). The patent describes no further firing.

Benötigte Werkzeuge:

Hydraulische PresseHydraulische Presse
Scheiben-PressformScheiben-Pressform
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Benötigte Werkzeuge:

ElektromagnetElektromagnet
KompassKompass

Materialien

3

Benötigte Werkzeuge

14

Dieser Bauplan stellt her

Verwandte Blueprints

Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...