Barium Ferrite Disc Magnet from Natural Magnetite, Presintered at 900 °C (Went, Philips 1956, Ex. 36, Procedure 1)
Charlie

Erstellt von

Charlie

28. Oktober 2026DE
2
0
0
0
0

Barium Ferrite Disc Magnet from Natural Magnetite, Presintered at 900 °C (Went, Philips 1956, Ex. 36, Procedure 1)

A barium ferrite magnet made from natural magnetite instead of ferric oxide: barium carbonate and magnetite ground 18 hours, presintered 3 hours at 900 °C, ground again 18 hours, pressed and sintered 2 hours at 1200 °C. Went's rod held 1,450 gauss with a coercive force of 2,425 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 36. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Erfahren
2 days

Anweisungen

1

Weigh barium carbonate and magnetite

Weigh 9.9 g barium carbonate (0.05 mol) and 46.9 g natural magnetite, Fe3O4 (0.20 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Materialien für diesen Schritt:

Bariumcarbonat (Witherit)Bariumcarbonat (Witherit)9.9 g
MagnetitMagnetit46.9 g

Benötigte Werkzeuge:

BalkenwaageBalkenwaage
GummihandschuheGummihandschuhe
P100-AtemschutzmaskeP100-Atemschutzmaske
2

Grind 18 hours in a ball mill

Grind the mixture in a ball mill for 18 hours. The patent does not say whether wet or dry.

Benötigte Werkzeuge:

EisenkugelmühleEisenkugelmühle
P100-AtemschutzmaskeP100-Atemschutzmaske
3

Presinter at 900 °C for 3 hours

Fire the ground mixture at 900 °C for three hours and let it cool.

Benötigte Werkzeuge:

MuffelofenMuffelofen
Tiegel mit Deckel (Porzellan)Tiegel mit Deckel (Porzellan)
TiegelzangeTiegelzange
Hitzebeständige HandschuheHitzebeständige Handschuhe
4

Grind 18 hours in a ball mill

Grind it again in a ball mill for 18 hours. The patent does not say whether wet or dry.

Benötigte Werkzeuge:

EisenkugelmühleEisenkugelmühle
P100-AtemschutzmaskeP100-Atemschutzmaske
5

Press at 1.5 t/cm²

Press at 1.5 tonnes per cm² (ours: discs instead of a rod).

Benötigte Werkzeuge:

Hydraulische PresseHydraulische Presse
Scheiben-PressformScheiben-Pressform
6

Sinter at 1200 °C for 2 hours

Sinter at 1200 °C for 2 hours. The patent gives no atmosphere for this example. Went's rod: 1,450 gauss, 2,425 oersted.

Benötigte Werkzeuge:

MuffelofenMuffelofen
TiegelzangeTiegelzange
Hitzebeständige HandschuheHitzebeständige Handschuhe
7

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Benötigte Werkzeuge:

ElektromagnetElektromagnet
KompassKompass

Materialien

2

Benötigte Werkzeuge

12

Dieser Bauplan stellt her

Verwandte Blueprints

Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...