Barium Ferrite Disc Magnet: 0.5 mol BaCO3 to 3.5 mol Iron Oxide, 10 Minutes at 1330 °C (Went, Philips 1956, Ex. 4)
Charlie

Erstellt von

Charlie

28. Oktober 2026DE
1
0
0
0
0

Barium Ferrite Disc Magnet: 0.5 mol BaCO3 to 3.5 mol Iron Oxide, 10 Minutes at 1330 °C (Went, Philips 1956, Ex. 4)

A barium ferrite with much more iron oxide: 0.5 mol barium carbonate to 3.5 mol, milled 15.5 hours, bound, formed and sintered 10 minutes at 1330 °C. Went's rod held 2,040 gauss with a coercive force of 2,380 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 4. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Erfahren
2 days

Anweisungen

1

Weigh barium carbonate and iron oxide

Weigh 99.2 g barium carbonate (0.5 mol) and 564.8 g ferric oxide (3.5 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Materialien für diesen Schritt:

Bariumcarbonat (Witherit)Bariumcarbonat (Witherit)99.2 g
Eisen(III)-oxidEisen(III)-oxid564.8 g

Benötigte Werkzeuge:

BalkenwaageBalkenwaage
GummihandschuheGummihandschuhe
P100-AtemschutzmaskeP100-Atemschutzmaske
2

Mill with alcohol 15.5 hours, dry and sieve

Grind the mixture with alcohol in a ball mill for 15.5 hours, then dry it and sieve it.

Benötigte Werkzeuge:

EisenkugelmühleEisenkugelmühle
Ethanol in Laborqualität, 95 %Ethanol in Laborqualität, 95 %
TrockenofenTrockenofen
WurfsiebWurfsieb
3

Knead with a binder and form

Mix 300 g of the powder with a binder such as polyvinyl alcohol (Went names it or nitrocellulose) into a kneadable mass. The patent extrudes rods about 3 mm across; ours: press discs at 1.5 tonnes per cm², as in its other examples. Dry them in air for about 24 hours.

Benötigte Werkzeuge:

Polyvinylalkohol-PulverPolyvinylalkohol-Pulver
Hydraulische PresseHydraulische Presse
Scheiben-PressformScheiben-Pressform
TrockenofenTrockenofen
4

Sinter in air at 1330 °C for 10 minutes

Sinter the pieces in air at 1330 °C for 10 minutes. The patent gives no zone length or speed for this example.

Benötigte Werkzeuge:

RohrofenRohrofen
Hitzebeständige HandschuheHitzebeständige Handschuhe
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Benötigte Werkzeuge:

ElektromagnetElektromagnet
KompassKompass

Materialien

2

Benötigte Werkzeuge

14

Dieser Bauplan stellt her

Verwandte Blueprints

Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...