Bismuth: Sweated Out of Native Ore in Inclined Iron Tubes, the Schneeberg Way (Thorpe, 1912)
Charlie

Erstellt von

Charlie

4. November 2026DE
6
0
0
0
0

Bismuth: Sweated Out of Native Ore in Inclined Iron Tubes, the Schneeberg Way (Thorpe, 1912)

The old way of getting bismuth from ore that holds it as the metal: heat the lumps just enough in sloping iron tubes and the bismuth, which melts easily, runs out of the rock into pots under charcoal. It takes 30-60 minutes a charge but gets only about two-thirds of the metal. Not given: the furnace temperature. Source: E. Thorpe, Dictionary of Applied Chemistry vol. I (1912), Bismuth, p. 458. Picture: Thorpe's Fig. 1, the furnace in plan.
Fortgeschritten
30-60 minutes per charge

Anweisungen

1

Pick and break the ore

Sort the ore (7-12 % bismuth) by hand from the waste rock as far as possible and break it into pieces the size of a hazel nut.

Materialien für diesen Schritt:

Gediegenes WismuterzGediegenes Wismuterz1 12 cwt per tube charge

Benötigte Werkzeuge:

HammerHammer
Industrie-PlattformwaageIndustrie-Plattformwaage
2

Charge the tubes

Load about 12 cwt into each inclined iron tube of the furnace, leaving room to stir from the upper end. Close the upper ends with iron plates and the lower ends with plates pierced with round holes. Under each lower end stand an iron pot holding powdered charcoal, kept gently warm by a small charcoal fire.

Materialien für diesen Schritt:

HolzkohleHolzkohle1 powdered, in the pots and for the pot fire

Benötigte Werkzeuge:

Wismut-SaigerofenWismut-Saigerofen
EisentiegelEisentiegel
3

Sweat out the bismuth

Fire the furnace with wood so that the metal flows easily. In about 10 minutes the bismuth begins to run into the pots, where the charcoal covers it from the air. Stir the ore now and then with an iron rod from the upper end; in 30-60 minutes the charge is done. 20 cwt of ore burns about 63 cubic feet of wood.

Materialien für diesen Schritt:

BrennholzBrennholz1 about 63 cu ft per 20 cwt of ore

Benötigte Werkzeuge:

Wismut-SaigerofenWismut-Saigerofen
EisenstabEisenstab
4

Rake out and recharge

Rake the spent ore (bismuth barley) out of the upper end into the tank and refill at once with fresh ore.

Benötigte Werkzeuge:

EisenrechenEisenrechen
Wismut-SaigerofenWismut-Saigerofen
5

Cast ingots

Ladle the bismuth from the pots into moulds and cast ingots of 25-50 lb.

Benötigte Werkzeuge:

EisentiegelEisentiegel
GießpfanneGießpfanne
BarrenkokilleBarrenkokille

Materialien

3
  • 1 12 cwt per tube charge
    Platzhalter
  • 1 powdered, in the pots and for the pot fire
    Platzhalter
  • 1 about 63 cu ft per 20 cwt of ore
    Platzhalter

Benötigte Werkzeuge

8

Dieser Bauplan stellt her

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...