Butyraldehyde: Butyl Alcohol Dehydrogenated over Copper Pellets at 400-680 °F (Hasche, Eastman, US 2,173,111)
Charlie

Erstellt von

Charlie

31. Oktober 2026DE
0
0
0
0
0

Butyraldehyde: Butyl Alcohol Dehydrogenated over Copper Pellets at 400-680 °F (Hasche, Eastman, US 2,173,111)

Hot copper pulls two hydrogen atoms off butyl alcohol and leaves butyraldehyde. Hasche's catalyst is copper made from blown, water-quenched cuprous oxide, in dust-free pellets that can be burnt clean and reduced again when they tire. Result: butyraldehyde, distilled off from the unchanged alcohol. Source: Hasche, US 2,173,111 (Eastman Kodak, 1939), claims 6, 9 and 12. His worked run is for propyl alcohol; conversion for butanol is not given. Picture drawn by Youblob.
Erfahren
1 day

Anweisungen

1

Pack the copper catalyst

Fill a tube with dust-free copper pellets made from cuprous oxide blown from molten copper and quenched in water (2-5 mesh in claim 17).

Benötigte Werkzeuge:

Kupfer-KatalysatorkörnerKupfer-Katalysatorkörner
RohrofenRohrofen
2

Preheat the butyl alcohol

Vaporise and preheat the butyl alcohol to about 500-600 °F.

Materialien für diesen Schritt:

n-Butanoln-Butanol1 as required

Benötigte Werkzeuge:

RohrofenRohrofen
3

Pass it over the copper at 400-680 °F

Lead the hot vapour over the catalyst held at about 400-680 °F. It splits into butyraldehyde and hydrogen; part of the alcohol passes unchanged.

Benötigte Werkzeuge:

Kupfer-KatalysatorkörnerKupfer-Katalysatorkörner
RohrofenRohrofen
KondensatorschlangeKondensatorschlange
4

Distil off the aldehyde

Condense the products and distil: butyraldehyde comes over first (it boils near 74 °C); distil the alcohol back in the presence of alkali and return it.

Benötigte Werkzeuge:

FraktionierbrennblaseFraktionierbrennblase
Natronlauge, 10-prozentige LösungNatronlauge, 10-prozentige Lösung
5

Reactivate the spent copper

When the catalyst slows, flush it, oxidise it at about 600-800 °F, cool, and reduce it again with alcohol vapour at about 300-400 °F.

Benötigte Werkzeuge:

Kupfer-KatalysatorkörnerKupfer-Katalysatorkörner
RohrofenRohrofen

Materialien

1
  • 1 as required
    Platzhalter

Benötigte Werkzeuge

5

Dieser Bauplan stellt her

Verwandte Blueprints

Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...