Ceramic Disc Capacitors: Barium Titanate with Nickel Stannate, Pressed, Fired and Silvered (Coffeen, US 2,789,061)
Ed

Erstellt von

Ed

2. November 2026FI
12
0
0
0
0

Ceramic Disc Capacitors: Barium Titanate with Nickel Stannate, Pressed, Fired and Silvered (Coffeen, US 2,789,061)

Barium titanate with 3 mole % nickel stannate is calcined, pressed into small discs and fired hard. Silver is fired onto both faces and a lead soldered to each, giving ceramic disc capacitors of high capacity for their size. Result: discs 3/8 inch across and about 1/10 inch thick with a dielectric constant averaging 2380 and a dissipation factor of 0.58 %. Between 25 and 85 °C the dielectric constant rose at most 17 % and fell at most 7 %. Source: W. W. Coffeen (Metal & Thermit Corp.), US 2,789,061 (1957). Unknown: how the barium titanate, the nickel stannate and the tinned lead wire are made; the patent uses them ready-made. Picture: Wikimedia Commons.
Erfahren
10 days

Anweisungen

1

Weigh and slurry

Weigh 19.32 g of barium titanate and 0.68 g of hydrated nickel stannate (about NiSnO3·2H2O), which is 97 mole % BaTiO3 and 3 mole % NiSnO3. Slurry them with 50 cc of distilled water. The patent prefers 2 to 4 mole % nickel stannate; 1 to 15 % works.

Materialien für diesen Schritt:

BariumtitanatBariumtitanat19.32 g
NickelstannatNickelstannat0.68 g

Benötigte Werkzeuge:

Destilliertes WasserDestilliertes Wasser
Digitale PräzisionswaageDigitale Präzisionswaage
AbdampfschaleAbdampfschale
2

Dry, sieve and calcine

Dry the slurry, crush it to pass a 50 mesh screen, moisten it with 5 % of a 2 1/2 % starch solution and press it into one slug. Calcine the slug for one hour at 1600 °F (871 °C). Ours: potato starch, a drying oven, mortar and pestle.

Benötigte Werkzeuge:

KartoffelstärkeKartoffelstärke
TrockenofenTrockenofen
Mörser und PistillMörser und Pistill
WurfsiebWurfsieb
Hydraulische PresseHydraulische Presse
HochbrandofenHochbrandofen
3

Press the discs

Grind the calcine to pass a 325 mesh screen, moisten it again with starch solution, and press small discs 3/8 inch in diameter and about 1/10 inch thick at 20,000 pounds per square inch.

Benötigte Werkzeuge:

Mörser und PistillMörser und Pistill
Feinmaschiges SiebFeinmaschiges Sieb
KartoffelstärkeKartoffelstärke
Hydraulische PresseHydraulische Presse
Scheiben-PressformScheiben-Pressform
4

Fire on platinum

Fire the discs on platinum foil at 2400 °F (1316 °C) for one hour. They come out with zero absorption.

Benötigte Werkzeuge:

HochbrandofenHochbrandofen
PlatinPlatin
5

Silver and lead

Paint silver paint on both faces and fire the discs at 1350 °F (732 °C) for one hour. Solder tinned copper lead wires directly to the silver electrodes. Age at least a week before measuring. Ours: a fine brush and a soldering iron.

Materialien für diesen Schritt:

Einbrenn-SilberleitlackEinbrenn-Silberleitlack1 both faces
Verzinnter KupferdrahtVerzinnter Kupferdraht2 leads per disc
LötdrahtLötdraht1 a little

Benötigte Werkzeuge:

Feinspitzige PinselFeinspitzige Pinsel
HochbrandofenHochbrandofen
LötkolbenLötkolben

Materialien

5

Benötigte Werkzeuge

14

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...