Continuous Glass Fibre Strand Drawn from a Platinum Bushing
Charlie

Erstellt von

Charlie

19. Oktober 2026DE
4
0
0
0
0

Continuous Glass Fibre Strand Drawn from a Platinum Bushing

Glass fibre for cloth is not spun like wool: hundreds of fine filaments are pulled at once from small nozzles in a hot platinum box and wound up as one strand. This is the method of Slayter and Thomas's Owens-Corning patent (US 2,234,986, 1941): an electrically heated platinum-rhodium thimble melts glass cullet, a blower freezes each filament just below its nozzle, a size is put on, and a drum pulls and winds the strand. The faster the drum, the finer the fibre. The picture: a glass fibre roving (NoiseD, Wikimedia Commons, CC BY-SA 3.0).
Erfahren
1 day

Anweisungen

1

Charge the bushing with cullet

Fill the platinum-rhodium thimble (90 % platinum, 10 % rhodium) with broken soda-lime glass. Its floor has rows of staggered nipples .02–.08 in (0.5–2 mm) wide; .04 in (1 mm) is best.

Materialien für diesen Schritt:

Kalk-Natron-GlasscherbenKalk-Natron-Glasscherben1 as required

Benötigte Werkzeuge:

Platin-Rhodium-DüsenwannePlatin-Rhodium-Düsenwanne
Hitzebeständige HandschuheHitzebeständige Handschuhe
SchutzbrilleSchutzbrille
2

Melt it with an electric current

Pass an adjustable current through the thimble to melt the glass. Ordinary lime glass is pulled from about 2,100–2,500 °F (about 1,150–1,370 °C).

Benötigte Werkzeuge:

Platin-Rhodium-DüsenwannePlatin-Rhodium-Düsenwanne
AbwärtstransformatorAbwärtstransformator
PyrometerPyrometer
Hitzebeständige HandschuheHitzebeständige Handschuhe
3

Start the cooling blower

Blow cool air across the nipple tips from a blower a short distance below them. Each filament sets within a small fraction of an inch of its nipple.

Benötigte Werkzeuge:

GebläseGebläse
4

Gather the filaments through a sized guide

Draw all the filaments together through one guide eye kept wet with size. Here the size is wax, kept molten with a burner; the patent also names oil, starch, gum and resin. An air jet dries off the excess size.

Materialien für diesen Schritt:

ParaffinParaffin1 as required

Benötigte Werkzeuge:

BunsenbrennerBunsenbrenner
GebläseGebläse
5

Pull and wind on a drum

Wind the strand on a fast drum that moves back and forth so it lays evenly. Draw at a few hundred to a few thousand feet per minute: the faster you draw, the finer the fibre.

Benötigte Werkzeuge:

AufwickeltrommelAufwickeltrommel

Materialien

2

Benötigte Werkzeuge

8

Dieser Bauplan stellt her

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...