Ebonite (Hard Rubber)

Vulcanised rubber is rubber with a few sulphur bridges between its chains. Keep adding sulphur and the bridges multiply until the chains cannot move at all: the soft, stretchy material turns into a hard black solid you can turn on a lathe, polish like ebony and use as an electrical insulator. **US 8,075**, "Improvement in the Manufacture of India Rubber", Nelson Goodyear (brother of Charles), granted 6. May 1851, claims "the combining of india-rubber and sulphur… for making a hard and inflexible substance hitherto unknown": about equal parts by weight, heated to 260–275 °F for three to six hours. It was one of the first rigid materials made by chemically changing a natural polymer, over half a century before Bakelite. **You turn a part from commercial ebonite rod and measure what the sulphur did** — its density, and its charge when rubbed. Curing ebonite needs a heated press and releases hydrogen sulphide, so the blueprint starts from finished rod; the notebook does the chemistry.
Fortgeschritten
3 hours

Anweisungen

1

Cut the blank

Clamp 20 mm ebonite rod in the vise between soft jaws. Saw off 60 mm. Ebonite chips like hard wood; saw slowly to avoid cracking the end.

Materialien für diesen Schritt:

EbonitstabEbonitstab1 Stück

Benötigte Werkzeuge:

Bügelsäge (Metallsäge)Bügelsäge (Metallsäge)
SchraubstockSchraubstock
StahllinealStahllineal
Klare SchutzbrilleKlare Schutzbrille
2

Chuck and face

Grip 20 mm of the blank in the lathe's 3-jaw chuck. Face the end square with a sharp HSS tool at about 800 rpm, light cuts.

Benötigte Werkzeuge:

MetalldrehmaschineMetalldrehmaschine
Drechselwerkzeug-Set (HSS)Drechselwerkzeug-Set (HSS)
Klare SchutzbrilleKlare Schutzbrille
StaubmaskeStaubmaske
3

Turn to 16 mm

Turn 40 mm of length down to 16.0 mm. Check with the caliper every pass. The chips smell of sulphur - that is the bonded sulphur you measure later.

Benötigte Werkzeuge:

MetalldrehmaschineMetalldrehmaschine
Drechselwerkzeug-Set (HSS)Drechselwerkzeug-Set (HSS)
Digitaler Messschieber 6 ZollDigitaler Messschieber 6 Zoll
4

Drill the bore

Spot the centre with a centre drill, then drill 3 mm through 35 mm from the tailstock. Clear chips every 5 mm - ebonite heats and gums if packed.

Benötigte Werkzeuge:

Satz ZentrierbohrerSatz Zentrierbohrer
Bohrersatz im KassettenkastenBohrersatz im Kassettenkasten
MetalldrehmaschineMetalldrehmaschine
5

Taper the grip

Set the compound to a shallow angle and taper 25 mm from 16 mm down to 10 mm. This is a fountain-pen grip section, the job ebonite still does today.

Benötigte Werkzeuge:

MetalldrehmaschineMetalldrehmaschine
Drechselwerkzeug-Set (HSS)Drechselwerkzeug-Set (HSS)
Digitaler Messschieber 6 ZollDigitaler Messschieber 6 Zoll
6

Sand and polish

At low speed, sand 400 then 800 grit, then run the Micro-Mesh grits in order. Finish with polishing compound on a cloth. Ebonite takes a deep gloss without lacquer.

Materialien für diesen Schritt:

SchleifpapierSchleifpapier2 Blätter
PolierpastePolierpaste5 g

Benötigte Werkzeuge:

Mikrogewebe-Schleifset (9 Körnungen)Mikrogewebe-Schleifset (9 Körnungen)
MetalldrehmaschineMetalldrehmaschine
StaubmaskeStaubmaske
7

Part off

Part off at 45 mm with the parting tool. Chamfer the cut end by hand with 800 grit.

Benötigte Werkzeuge:

Drechselwerkzeug-Set (HSS)Drechselwerkzeug-Set (HSS)
MetalldrehmaschineMetalldrehmaschine
8

Measure the density

Weigh the part. Drop it into 50 ml of water in the graduated cylinder and read the rise. Do the same with a bundle of rubber bands. Enter both in the notebook.

Materialien für diesen Schritt:

GummibänderGummibänder1 Packung

Benötigte Werkzeuge:

Digitale PräzisionswaageDigitale Präzisionswaage
MesszylinderMesszylinder
9

Rub it and pick up paper

Tear tissue into 5 mm scraps. Rub the ebonite 10 strokes on wool felt and hold it 2 cm above the scraps. Repeat with an acrylic offcut. Count scraps lifted by each.

Materialien für diesen Schritt:

Säurefreies SeidenpapierSäurefreies Seidenpapier1 Blatt
AcrylplatteAcrylplatte1 Stück

Benötigte Werkzeuge:

WollfilzWollfilz
10

The sulphur arithmetic

Jupyter-Notebook wird geladen …
11

History & Context

**What the patent specifies:** rubber and sulphur in about equal parts (or 2 : 1 with magnesia or lime), 260–275 °F, three to six hours. **Modern build (derived):** commercial ebonite rod, typically 25–32 % sulphur - the notebook shows why more than about 32 % cannot bond. Ebonite was named for ebony, which it replaced in combs, pipe stems and instrument parts. It became a standard insulator of the electrical age and is still preferred for fountain-pen feeds because ink wets it. Its limits: it softens with heat, fades to brown and smells of sulphur in sunlight as the surface oxidises, and is brittle under impact.

Materialien

6

Benötigte Werkzeuge

14

Verwandte Blueprints

Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...