Electrolytic Iron: Brown Ferrous Electrolyte, Rotating Cathode at 75-77 °C, Graphite Anodes (Bouchayer, US 1,516,326)

Iron plated out of a fresh green ferrous bath comes off rough and useless. Bouchayer first stirred the bath in air until it turned bright brown; the iron oxychloride formed takes care of the hydrogen at the cathode, and the deposit grows even and compact at high current. Result: electrolytic iron, deposited at about 98 % current yield. Source: Bouchayer, US 1,516,326 (1924). Not given: cathode material, purity of the iron. Picture drawn by Youblob.
Erfahren
Factory process

Anweisungen

1

Make up the electrolyte at 20 °Bé

Dissolve ferrous sulfate in water (Bouchayer also allows ferrous chloride or a mix). Concentration: e.g. 20 °Bé, then keep it constant.

Materialien für diesen Schritt:

EisensulfatEisensulfat1 as required

Benötigte Werkzeuge:

WasserWasser
Spindel (Aräometer)Spindel (Aräometer)
ElektrolysebehälterElektrolysebehälter
2

Stir it in air until brown

Agitate the green bath in air, e.g. by turning the anode, until it is bright brown and stops foaming. Used green, it gives only an irregular deposit.

Benötigte Werkzeuge:

ElektrolysebehälterElektrolysebehälter
3

Circulate it through iron filings

Pump the electrolyte through a mass of iron filings in a separate vessel; it takes back iron and forms the ferric hydroxide that keeps the bath working. Keep it moving fast past the anodes: this lowers the phosphorus.

Materialien für diesen Schritt:

EisenspäneEisenspäne1 as required

Benötigte Werkzeuge:

WasserpumpeWasserpumpe
4

Deposit on a rotating cathode

Electrolyse between graphite anodes and a rotating cathode. Temperature: e.g. 75-77 °C at 1000 A/m², held exactly constant and below boiling; cathode speed: e.g. 120 m/min at 800 A/m². Cathode material: not given.

Benötigte Werkzeuge:

GrafitelektrodeGrafitelektrode
GleichstromnetzgerätGleichstromnetzgerät
ThermometerThermometer
ElektrolysebehälterElektrolysebehälter
5

Strip and reheat the deposit

Take the compact iron deposit off the cathode; it is usable after a slight reheating (temperature not given).

Benötigte Werkzeuge:

ElektrolysebehälterElektrolysebehälter

Materialien

2
  • 1 as required
    Platzhalter
  • 1 as required
    Platzhalter

Benötigte Werkzeuge

7

Dieser Bauplan stellt her

Verwandte Blueprints

Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...