Extruded Polystyrene Foam: Propylene-Blown Log Let Out at 50 °C (McIntire, Dow 1948, Ex. 3, Test 2)
Charlie

Erstellt von

Charlie

28. Oktober 2026DE
6
0
0
0
0

Extruded Polystyrene Foam: Propylene-Blown Log Let Out at 50 °C (McIntire, Dow 1948, Ex. 3, Test 2)

Extruded polystyrene foam blown with a propylene gas fraction instead of methyl chloride. Polystyrene stands two days at 40 °C with the propylene under pressure and becomes a gel. Let out at 50 °C (250 psi in the tower), it swelled into a log 6 to 9 inches across, weighing 4.8 lb per cubic foot, with somewhat smaller, uniform cells. Source: O. R. McIntire (Dow), US 2,450,436 (1948), Example 3. Picture: the patent's drawing.
Erfahren
3 days

Anweisungen

1

Charge the tower with polystyrene

Charge a high-pressure tower with 300 lb of granular polystyrene.

Materialien für diesen Schritt:

PolystyrolPolystyrol300 lbs

Benötigte Werkzeuge:

DruckreaktorDruckreaktor
BalkenwaageBalkenwaage
GummihandschuheGummihandschuhe
2

Add the propylene fraction

Add 100 lb of a cracked-oil gas fraction that is about 93 % propylene, under pressure, and close the tower. Propylene is a flammable gas: no flames, strong ventilation.

Materialien für diesen Schritt:

PropylenPropylen100 lbs

Benötigte Werkzeuge:

DruckgasflascheDruckgasflasche
DruckreaktorDruckreaktor
ChemikalienschutzbrilleChemikalienschutzbrille
3

Stand two days at 40 °C

Let the tower stand for two days at 40 °C while the polystyrene takes up the propylene.

Benötigte Werkzeuge:

DruckreaktorDruckreaktor
LaborthermometerLaborthermometer
4

Let it out at 50 °C

Open the valved outlet near the bottom (3.25 inch in the patent) at 50 °C. The pressure is about 250 psi. The gel flows out and swells into a log 6 to 9 inches across, 4.8 lb per cubic foot, with somewhat smaller, uniform cells. Close the outlet again. The patent heated step by step (50, 60, 75 °C) for several hours each, letting a portion out at each step.

Benötigte Werkzeuge:

DruckreaktorDruckreaktor
LaborthermometerLaborthermometer
ChemikalienschutzbrilleChemikalienschutzbrille
GummihandschuheGummihandschuhe
5

Saw into boards

When the foam has set, saw it lengthwise into slabs (ours: a woodworking saw).

Benötigte Werkzeuge:

TischlersägeTischlersäge
GummihandschuheGummihandschuhe

Materialien

2
  • 300 lbs
    Platzhalter
  • 100 lbs
    Platzhalter

Benötigte Werkzeuge

7

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.