3D Printer Filament Extruded from Pellets
Pixel

Erstellt von

Pixel

11. Oktober 2026FI
45
0
0
0
0

3D Printer Filament Extruded from Pellets

Filament is made the way a 3D printer prints, only continuously: dry plastic pellets fall from a hopper onto a turning screw inside a heated barrel, melt as they are carried forward, and are pushed out through a round nozzle. The strand is cooled in air or a water bath, drawn by a puller at a steady speed so it keeps its diameter, and wound on a spool. Commercial 1.75 mm filament is typically held to about ±0.02 mm; a small line should be measured. PETG and many other plastics take up moisture, which makes bubbles and weak prints: makers dry PETG at about 55–70 °C for 5–8 hours, depending on the resin. Melt temperatures follow the resin's datasheet; PETG is usually printed at about 230–260 °C.
Fortgeschritten
A day per few kilograms

Anweisungen

1

Dry the pellets

Dry the pellets in a dryer as the resin maker specifies; for PETG about 55–70 °C for 5–8 hours.

Materialien für diesen Schritt:

PETG-GranulatPETG-Granulat2 kg
Biologisch abbaubares Kunststoffgranulat (PLA)Biologisch abbaubares Kunststoffgranulat (PLA)2 kg
ABS-GranulatABS-Granulat2 kg

Benötigte Werkzeuge:

GranulattrocknerGranulattrockner
Digitale KüchenwaageDigitale Küchenwaage
2

Heat the barrel

Set the barrel's heating zones to rise from the hopper end to the nozzle within the resin's datasheet range and let them settle.

Benötigte Werkzeuge:

Einschnecken-ExtruderzylinderEinschnecken-Extruderzylinder
PelletzuführtrichterPelletzuführtrichter
3

Extrude

Fill the hopper and start the screw slowly. Purge until the strand comes out clear of old material and bubbles.

Benötigte Werkzeuge:

Einschnecken-ExtruderzylinderEinschnecken-Extruderzylinder
PelletzuführtrichterPelletzuführtrichter
Hitzebeständige HandschuheHitzebeständige Handschuhe
SchutzbrilleSchutzbrille
4

Cool and pull

Lead the strand through a water bath or past the fan to the puller. Adjust the puller's speed: faster pulls the strand thinner, slower lets it swell.

Materialien für diesen Schritt:

WasserWasser50 Liter

Benötigte Werkzeuge:

Große Kunststoffwanne, 100 lGroße Kunststoffwanne, 100 l
Kastenventilator (stufenlos)Kastenventilator (stufenlos)
Filamentabzug und -wicklerFilamentabzug und -wickler
5

Measure and wind

Measure the diameter every few metres and wind the filament on a spool. Keep it sealed and dry.

Benötigte Werkzeuge:

Digitaler Messschieber 6 ZollDigitaler Messschieber 6 Zoll
Filamentabzug und -wicklerFilamentabzug und -wickler
Digitale KüchenwaageDigitale Küchenwaage
6

Troubleshooting

Filament extrusion troubleshooting.

Flow

Loading...

Materialien

4

Benötigte Werkzeuge

10

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...