Fireclay Firebricks

Firebricks line kilns, forges and furnaces because they stand heat that would slump or crack ordinary brick. They are refractory fireclay bound round a large share of grog. Potters' guides give about 20–40 % grog for general kiln bricks and up to 60–80 % for the hottest parts such as fireboxes; the bonding clay should be a little less refractory than the grog. Factory firebricks are fired at about 1,100–1,400 °C. Make test bricks first, fire them, and check them for cracks before making a whole batch.
Fortgeschritten
A day, plus weeks drying and a firing

Anweisungen

1

Choose the mix

For general kiln walls weigh about 70 parts fireclay to 30 parts coarse grog; for a firebox about 30 to 70. Write the mix on a label.

Benötigte Werkzeuge:

WaageWaage
2

Mix

Mix the dry fireclay and grog in the trough, then add water a little at a time and tread or turn it until it is stiff and holds together.

Materialien für diesen Schritt:

SchamottetonSchamotteton14 kg
Schamotte (gemahlene Scherben)Schamotte (gemahlene Scherben)6 kg
WasserWasser3 Liter

Benötigte Werkzeuge:

MörteltrogMörteltrog
SpatenSpaten
StaubmaskeStaubmaske
3

Mould

Dust the wet brick mould with sand, throw a lump in hard so it fills the corners, strike off the top with the straightedge and tip the brick out onto a board.

Materialien für diesen Schritt:

SandSand1 kg

Benötigte Werkzeuge:

Ziegelform aus HolzZiegelform aus Holz
HaarlinealHaarlineal
4

Dry slowly

Dry the bricks on pallets under cover, out of sun and wind, for several weeks, turning them now and then. They must be dry right through before firing.

Benötigte Werkzeuge:

HolzpaletteHolzpalette
PlanePlane
5

Fire

Stack them with gaps in the kiln and fire them slowly at first, then as hot as the kiln will safely go. Note the top temperature on the pyrometer.

Benötigte Werkzeuge:

BrennofenBrennofen
PyrometerPyrometer
BrennhilfsmittelBrennhilfsmittel
6

Check them

When cold, tap each brick: a clear ring means it is sound, a dull thud means a crack. Measure the shrinkage for the next batch.

Benötigte Werkzeuge:

Bandmaß (Rollmeter)Bandmaß (Rollmeter)
7

Troubleshooting

Firebrick troubleshooting.

Flow

Loading...

Materialien

4

Benötigte Werkzeuge

12

Verwandte Blueprints

Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...