A small one-handed axe forged from a 7/8 × 2-inch bar of good tool steel, best made by two people; a 6¾-inch bar gives two heads. The eye, about 9/16 × 1½ inches, is punched at a yellow heat with an eye punch and opened with drifts, the blade drawn out to a 3-inch edge and the head cut to length. The axe is annealed in lime or ashes, ground and buffed, then hardened from the hardening heat in tepid water and tempered by two hot iron bars laid on either side at the centre: dark purple for the blade, blue for the head.
Erfahren
4–6 hours

Anweisungen

1

Mark and punch the eye

Mark the stock with chisel and centre punch. At a yellow heat, punch the eye with the narrow edge of the punch toward the blade; lift the punch after each blow to check it runs straight and to let it cool; a little fine coal in the hole stops it sticking. Punch nearly through, then finish from the other side.

Materialien für diesen Schritt:

Werkzeugstahl-FlachstabWerkzeugstahl-Flachstab1 Stück

Benötigte Werkzeuge:

KörnerKörner
SchmiedeesseSchmiedeesse
AmbossAmboss
WarmlocheisenWarmlocheisen
VorschlaghammerVorschlaghammer
SchmiedezangeSchmiedezange
2

Drift and draw out

Drive in a tool-steel drift, hammer the bulges down to the bar's size and smooth with a flatter; take the drift out before each reheat. Use two drifts, the first 3/8 inch narrower. Draw out the blade, driving the drift back in as the eye stretches so no cold shut forms.

Benötigte Werkzeuge:

LochdornLochdorn
Flachhammer-SetzeisenFlachhammer-Setzeisen
SchwanzhammerSchwanzhammer
3

Shape and trim

Shape the blade with a heavy hammer and flatter and form its edge. Cut the head from the bar, draw it to size, cut it to length, then trim the blade to shape.

Benötigte Werkzeuge:

SchmiedehammerSchmiedehammer
Flachhammer-SetzeisenFlachhammer-Setzeisen
WarmschrotmeißelWarmschrotmeißel
4

Anneal and grind

Heat to a full red and anneal in lime or ashes. When cold, grind on an emery wheel and finish on a buffing wheel.

Benötigte Werkzeuge:

SchmiedeesseSchmiedeesse
DoppelschleiferDoppelschleifer
5

Harden and temper

Heat very slowly to the hardening heat and cool in tepid water. Draw the temper with two hot iron bars laid on either side at the centre; when the blade is dark purple and the head blue, cool quickly in water.

Benötigte Werkzeuge:

SchmiedeesseSchmiedeesse
AbschreckbottichAbschreckbottich
SchmiedezangeSchmiedezange
6

Handle

Shave the handle stock to fit the eye tightly, drive the head on, saw a kerf in the handle's top and drive a glued hardwood wedge into it. Trim flush and oil the handle.

Materialien für diesen Schritt:

Hartholzstiel-RohlingHartholzstiel-Rohling1 Stück
HartholzkeilHartholzkeil1 Stück
LeinölLeinöl10 ml

Benötigte Werkzeuge:

SchweifhobelSchweifhobel
ZugsägeZugsäge
SchraubstockSchraubstock

Materialien

4

Benötigte Werkzeuge

16

Dieser Bauplan stellt her

Verwandte Blueprints

Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...