Hard Porcelain Body: Kaolin, Felspar, Flint and Chalk, the Sèvres Paste
Hard porcelain is white kaolin made just fusible enough with ground felspar. Andrew Ure (1839) gives the Sèvres paste: 63–70 parts washed kaolin, 22–15 felspar, about 10 flint powder and 5 chalk, mixed as slips, stiffened on plaster and left to ripen damp for months before it is trodden and used.
The picture: centring porcelain paste on the wheel in the Grand Atelier of the Sèvres manufactory.
Erfahren
Days to mix, months to ripen
Anweisungen
1
1
Calcine and grind the felspar
Calcine and grind the felspar
Pick felspar free of dark mica and rust. Heat it red hot in the kiln and quench it so it crumbles, then crush and grind it very fine with water and sift.
Materialien für diesen Schritt:
Feldspatbrocken2 kg
Wasser10 LiterBenötigte Werkzeuge:
Brennofen
Abschreckbottich
Mörser und Pistill
Läufer
Feinmaschiges Sieb
Hitzebeständige Handschuhe
Staubmaske2
2
Flint powder
Flint powder
Calcine and quench flint the same way and grind it to a fine powder with water.
Materialien für diesen Schritt:
Feuersteinknolle1 kgBenötigte Werkzeuge:
Brennofen
Abschreckbottich
Läufer
Feinmaschiges Sieb
Staubmaske3
3
Weigh and mix the slips
Weigh and mix the slips
Weigh the dry kaolin, felspar, flint and chalk in Ure's proportions, stir each into water and mix them into one smooth slip; pass it through a fine sieve.
Materialien für diesen Schritt:
Kaolinpulver6.65 kg
Calciumcarbonat (Schlämmkreide)0.5 kg
Wasser15 LiterBenötigte Werkzeuge:
Balkenwaage
Bütte
Feinmaschiges Sieb4
4
Stiffen on plaster, ripen
Stiffen on plaster, ripen
Pour the slip onto plaster bats to draw the water out without heat. When it is a soft paste, store it covered and damp for months to ripen.
Benötigte Werkzeuge:
Gipsscheibe für die Töpferei5
5
Tread and ball it
Tread and ball it
Before use, work the paste hard on the wedging table (Sèvres trod it barefoot) until even, and keep it in damp balls.
Benötigte Werkzeuge:
Schlagtisch für Ton6
6
Ure's Sèvres paste, scaled
Ure's Sèvres paste, scaled
Jupyter-Notebook wird geladen …
7
7
Limits
Limits
The recipe and handling are Ure's; calcining the flint and the batch size are ours. Grinding flint and felspar makes fine silica dust that harms the lungs over time: grind wet and wear a mask.
Materialien
5- 2 kgPlatzhalter
- 25 LiterPlatzhalter
- 1 kgPlatzhalter
- 6.65 kgPlatzhalter
- Platzhalter
Benötigte Werkzeuge
11- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
Dieser Bauplan stellt her
Verwandte Blueprints
Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien
CC0 Gemeinfrei
Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.
Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.