Lactide: Lactic Acid Condensed and Cracked under Vacuum, Recrystallised

Lactide is the ring-shaped double molecule of lactic acid, the monomer from which PLA is made. Schneider's du Pont patent (US 2,703,316, 1955) drives the water out of lactic acid, condenses it under vacuum to a syrupy low polymer, then heats that to 200–250 °C at 8–10 mm so that lactide distils off. For a tough plastic it must be very pure: recrystallise it from ethyl acetate until it melts at 120 °C or higher (best 123–125 °C). The picture: our diagram.
Erfahren
1–2 days

Anweisungen

1

Drive off the water

Distil the lactic acid at atmospheric pressure at 120–130 °C until nearly all the water of dilution has gone.

Materialien für diesen Schritt:

Milchsäure (technisch)Milchsäure (technisch)1 Stück

Benötigte Werkzeuge:

RundkolbenRundkolben
KondensatorschlangeKondensatorschlange
HeizplatteHeizplatte
ÖlbadÖlbad
LaborthermometerLaborthermometer
2

Condense under vacuum

Continue distilling under 17–35 mm of mercury. Water of esterification comes off and the acid becomes a syrupy low polymer (polylactic acid).

Benötigte Werkzeuge:

VakuumpumpeVakuumpumpe
VakuummeterVakuummeter
KühlfalleKühlfalle
ÖlbadÖlbad
LaborthermometerLaborthermometer
3

Crack to lactide

Lower the pressure to 8–10 mm and raise the temperature to 200–250 °C. Lactide distils at 130–140 °C (10–13 mm) and sets to a soft crystalline solid.

Benötigte Werkzeuge:

VakuumpumpeVakuumpumpe
VakuummeterVakuummeter
KondensatorschlangeKondensatorschlange
ÖlbadÖlbad
LaborthermometerLaborthermometer
Hitzebeständige HandschuheHitzebeständige Handschuhe
4

Recrystallise from ethyl acetate

Recrystallise the crude lactide from ethyl acetate, filter and dry. Repeat: in the patent the melting point rose from 114–115 °C after the first crystallisation to 118, 123–124 and 124–125 °C after the fourth.

Benötigte Werkzeuge:

EthylacetatEthylacetat
Hitzebeständiges BecherglasHitzebeständiges Becherglas
HeizplatteHeizplatte
Büchnertrichter (Porzellan)Büchnertrichter (Porzellan)
FilterpapierFilterpapier
ChemikalienschutzbrilleChemikalienschutzbrille
5

Check the melting point

Put a few crystals in a capillary tube and warm slowly. Lactide melting at 120 °C or above is fit for making PLA; below 120 °C it gives a brittle polymer.

Benötigte Werkzeuge:

Glas-KapillarrohrGlas-Kapillarrohr
LaborthermometerLaborthermometer
ÖlbadÖlbad

Materialien

1

Benötigte Werkzeuge

15

Dieser Bauplan stellt her

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...