Lithium salts from lepidolite by Troost's method: the powdered mineral is fused with barium carbonate, barium sulphate and potassium sulphate, the alkali sulphate layer turned into chlorides with barium chloride, and the lithium chloride dissolved out with alcohol and ether. The saline chlorides left behind are the residue in which Bunsen found rubidium.
The fusion separates into two layers: barium silicate and sulphate below, white potassium and lithium sulphate above.
Source: T. E. Thorpe, Dictionary of Applied Chemistry vol. III (1912), p. 338. Picture: the book's text.
Erfahren
Unknown
Anweisungen
1
1
Fuse with barium salts
Fuse with barium salts
Mix 10 parts finely powdered lepidolite with 10 parts barium carbonate, 5 parts barium sulphate and 3 parts potassium sulphate, and ignite at the highest heat of a wind furnace. Two layers form: barium silicate and sulphate below, white potassium and lithium sulphate above.
Materialien für diesen Schritt:
Lepidolith1 10 parts, finely powdered
Bariumcarbonat (Witherit)1 10 parts
Baryt (Schwerspat)1 5 parts
Kaliumsulfat1 3 partsBenötigte Werkzeuge:
Mörser und Pistill
Schmelztiegel
Holzkohle-Tiegelofen2
2
Turn the alkalis into chlorides
Turn the alkalis into chlorides
Lixiviate the upper layer with water and treat it with barium chloride, which turns the alkalis into chlorides and throws down the sulphuric acid as barium sulphate. Filter.
Materialien für diesen Schritt:
Bariumchlorid1 Stück
Wasser1 StückBenötigte Werkzeuge:
Filterpapier3
3
Take out the lithium chloride
Take out the lithium chloride
Evaporate the solution to dryness and digest with equal parts of absolute alcohol and ether: the lithium chloride dissolves with only a trace of potassium and sodium chloride. What stays undissolved is the saline residue of alkali chlorides.
Benötigte Werkzeuge:
Abdampfschale
Absoluter Alkohol
DiethyletherMaterialien
6- 1 10 parts, finely powderedPlatzhalter
- 1 10 partsPlatzhalter
- 1 5 partsPlatzhalter
- 1 3 partsPlatzhalter
- 1 StückPlatzhalter
- 1 StückPlatzhalter
Benötigte Werkzeuge
7- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
Dieser Bauplan stellt her
CC0 Gemeinfrei
Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.
Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.