Oriented Barium Ferrite Disc Magnet: Set in a 9500 Oersted Field (Gorter, Philips 1956, Ex. 1)
A ceramic magnet that is stronger in one direction. Pre-fired barium ferrite powder is suspended in polyvinyl acetate dissolved in acetone and set in a strong magnetic field, so its crystals line up. The block is heated to 500 °C in a weaker field and sintered at 1280 °C. In the principal direction it held 2,650 gauss with a coercive force of 1,775 oersted and a (BH)max of 1.3 × 10⁶; at right angles only 1,260 gauss.
Source: E. W. Gorter, G. W. Rathenau and A. L. Stuyts (Philips), US 2,762,778 (1956), Example 1. They made blocks; disc size is ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Erfahren
3 days
Anweisungen
1
1
Weigh barium carbonate and iron oxide
Weigh barium carbonate and iron oxide
Weigh 450 g barium carbonate and 2000 g ferric oxide. Barium carbonate is poisonous if swallowed: gloves and a dust respirator.
Materialien für diesen Schritt:
Bariumcarbonat (Witherit)450 g
Eisen(III)-oxid2000 gBenötigte Werkzeuge:
Balkenwaage
Gummihandschuhe
P100-Atemschutzmaske2
2
Mill 20 hours under alcohol, dry
Mill 20 hours under alcohol, dry
Grind the mixture in a ball mill under alcohol for 20 hours, then dry it.
Benötigte Werkzeuge:
Eisenkugelmühle
Ethanol in Laborqualität, 95 %
Trockenofen3
3
Pre-fire: through a 1100 °C zone in 10 minutes
Pre-fire: through a 1100 °C zone in 10 minutes
Pass the dry powder at 20 mm per minute through an electric furnace with a 20 cm hot zone at 1100 °C, in air: 10 minutes in the heat. Let it cool.
Benötigte Werkzeuge:
Rohrofen
Tiegel mit Deckel (Porzellan)
Hitzebeständige Handschuhe4
4
Grind 12 hours with alcohol, dry
Grind 12 hours with alcohol, dry
Pulverise the pre-fired material in a ball mill with alcohol for 12 hours, then dry it. This is the pre-fired powder.
Benötigte Werkzeuge:
Eisenkugelmühle
Ethanol in Laborqualität, 95 %
Trockenofen5
5
Stir into 16 % polyvinyl acetate in acetone
Stir into 16 % polyvinyl acetate in acetone
Dissolve polyvinyl acetate in acetone to a 16 % solution and stir the pre-fired powder into it, 2 cc of solution per gram of powder. The binder burns off later.
Benötigte Werkzeuge:
Polyvinylacetat
Aceton
Balkenwaage6
6
Orient in a 9500 oersted field
Orient in a 9500 oersted field
Put the suspension in a brass die between the poles of a magnet yoke and apply a first field of 9500 oersted. Let the acetone evaporate while the field is on. A small block forms.
Benötigte Werkzeuge:
Scheiben-Pressform
Elektromagnet
Hydraulische Presse7
7
Heat to 500 °C in a 2000 oersted field
Heat to 500 °C in a 2000 oersted field
Put the block in an electric furnace between the magnet's poles. With a second field of 2000 oersted along the first field's direction, heat to 500 °C, which burns off the rest of the binder. Then switch the field off.
Benötigte Werkzeuge:
Rohrofen
Elektromagnet
Hitzebeständige Handschuhe8
8
Sinter: through a 1280 °C zone in 5 minutes
Sinter: through a 1280 °C zone in 5 minutes
Pass the block at 20 mm per minute through an electric furnace in air at 1280 °C with a 10 cm hot zone: about 5 minutes in the heat.
Benötigte Werkzeuge:
Rohrofen
Hitzebeständige Handschuhe9
9
Magnetise in the principal direction
Magnetise in the principal direction
Magnetise the block along the direction of the first field, the principal direction. The patent magnetises it in a field in that direction; ours: an electromagnet. Find the north face with a compass.
Benötigte Werkzeuge:
Elektromagnet
KompassMaterialien
2- Platzhalter
- 2000 gPlatzhalter
Benötigte Werkzeuge
15- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
Dieser Bauplan stellt her
Verwandte Blueprints
Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien
CC0 Gemeinfrei
Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.
Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.