Oriented Barium Ferrite Disc Magnet: Binder Dried in a 2400 Oersted Field (Gorter, Philips 1956, Ex. 3)
Charlie

Erstellt von

Charlie

28. Oktober 2026DE
5
0
0
0
0

Oriented Barium Ferrite Disc Magnet: Binder Dried in a 2400 Oersted Field (Gorter, Philips 1956, Ex. 3)

A ceramic magnet from pre-fired barium ferrite in polyvinyl acetate and acetone, dried in a 2400 oersted field, then pressed, heated and sintered as in Example 2. In the principal direction it held 2,720 gauss with a coercive force of 1,620 oersted and a (BH)max of 1.2 × 10⁶; at right angles 1,610 gauss. Source: E. W. Gorter, G. W. Rathenau and A. L. Stuyts (Philips), US 2,762,778 (1956), Example 3. They made blocks; disc size is ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Erfahren
3 days

Anweisungen

1

Weigh barium carbonate and iron oxide

Weigh 450 g barium carbonate and 2000 g ferric oxide. Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Materialien für diesen Schritt:

Bariumcarbonat (Witherit)Bariumcarbonat (Witherit)450 g
Eisen(III)-oxidEisen(III)-oxid2000 g

Benötigte Werkzeuge:

BalkenwaageBalkenwaage
GummihandschuheGummihandschuhe
P100-AtemschutzmaskeP100-Atemschutzmaske
2

Mill 20 hours under alcohol, dry

Grind the mixture in a ball mill under alcohol for 20 hours, then dry it.

Benötigte Werkzeuge:

EisenkugelmühleEisenkugelmühle
Ethanol in Laborqualität, 95 %Ethanol in Laborqualität, 95 %
TrockenofenTrockenofen
3

Pre-fire: through a 1100 °C zone in 10 minutes

Pass the dry powder at 20 mm per minute through an electric furnace with a 20 cm hot zone at 1100 °C, in air: 10 minutes in the heat. Let it cool.

Benötigte Werkzeuge:

RohrofenRohrofen
Tiegel mit Deckel (Porzellan)Tiegel mit Deckel (Porzellan)
Hitzebeständige HandschuheHitzebeständige Handschuhe
4

Grind 12 hours with alcohol, dry

Pulverise the pre-fired material in a ball mill with alcohol for 12 hours, then dry it. This is the pre-fired powder.

Benötigte Werkzeuge:

EisenkugelmühleEisenkugelmühle
Ethanol in Laborqualität, 95 %Ethanol in Laborqualität, 95 %
TrockenofenTrockenofen
5

Stir into 8 % polyvinyl acetate in acetone

Dissolve polyvinyl acetate in acetone to a 8 % solution and stir the pre-fired powder into it, 2 cc of solution per gram of powder. The binder burns off later.

Benötigte Werkzeuge:

PolyvinylacetatPolyvinylacetat
AcetonAceton
BalkenwaageBalkenwaage
6

Orient in a 2400 oersted field

Put the suspension in a moulding die between the poles of a magnet and apply a first field of 2400 oersted. Remove the binder solution while the field is on.

Benötigte Werkzeuge:

Scheiben-PressformScheiben-Pressform
ElektromagnetElektromagnet
Hydraulische PresseHydraulische Presse
7

Compress into a block

Compress the powder into a block as in Example 2. The pressure is not given.

Benötigte Werkzeuge:

Hydraulische PresseHydraulische Presse
Scheiben-PressformScheiben-Pressform
8

Heat to 500 °C in a 2000 oersted field

Put the block in an electric furnace between the magnet's poles. With a second field of 2000 oersted along the first field's direction, heat to 500 °C, which burns off the rest of the binder. Then switch the field off.

Benötigte Werkzeuge:

RohrofenRohrofen
ElektromagnetElektromagnet
Hitzebeständige HandschuheHitzebeständige Handschuhe
9

Sinter: through a 1300 °C zone in 5 minutes

Pass the block at 20 mm per minute through an electric furnace in air at 1300 °C with a 10 cm hot zone: about 5 minutes in the heat.

Benötigte Werkzeuge:

RohrofenRohrofen
Hitzebeständige HandschuheHitzebeständige Handschuhe
10

Magnetise in the principal direction

Magnetise the block along the direction of the first field, the principal direction. The patent magnetises it in a field in that direction; ours: an electromagnet. Find the north face with a compass.

Benötigte Werkzeuge:

ElektromagnetElektromagnet
KompassKompass

Materialien

2

Benötigte Werkzeuge

15

Dieser Bauplan stellt her

Verwandte Blueprints

Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.