Oriented Barium Ferrite Disc Magnet: Heated to 500 °C Without a Field (Gorter, Philips 1956, Ex. 6)
Charlie

Erstellt von

Charlie

28. Oktober 2026DE
5
0
0
0
0

Oriented Barium Ferrite Disc Magnet: Heated to 500 °C Without a Field (Gorter, Philips 1956, Ex. 6)

A ceramic magnet oriented in the die as in Example 4, but heated to 500 °C with no second field before sintering at 1280 °C. In the principal direction it held 3,025 gauss with a coercive force of 1,550 oersted and a (BH)max of 1.58 × 10⁶. Source: E. W. Gorter, G. W. Rathenau and A. L. Stuyts (Philips), US 2,762,778 (1956), Example 6. They made blocks; disc size is ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Erfahren
3 days

Anweisungen

1

Weigh barium carbonate and iron oxide

Weigh 450 g barium carbonate and 2000 g ferric oxide. Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Materialien für diesen Schritt:

Bariumcarbonat (Witherit)Bariumcarbonat (Witherit)450 g
Eisen(III)-oxidEisen(III)-oxid2000 g

Benötigte Werkzeuge:

BalkenwaageBalkenwaage
GummihandschuheGummihandschuhe
P100-AtemschutzmaskeP100-Atemschutzmaske
2

Mill 20 hours under alcohol, dry

Grind the mixture in a ball mill under alcohol for 20 hours, then dry it.

Benötigte Werkzeuge:

EisenkugelmühleEisenkugelmühle
Ethanol in Laborqualität, 95 %Ethanol in Laborqualität, 95 %
TrockenofenTrockenofen
3

Pre-fire: through a 1100 °C zone in 10 minutes

Pass the dry powder at 20 mm per minute through an electric furnace with a 20 cm hot zone at 1100 °C, in air: 10 minutes in the heat. Let it cool.

Benötigte Werkzeuge:

RohrofenRohrofen
Tiegel mit Deckel (Porzellan)Tiegel mit Deckel (Porzellan)
Hitzebeständige HandschuheHitzebeständige Handschuhe
4

Grind 12 hours with alcohol, dry

Pulverise the pre-fired material in a ball mill with alcohol for 12 hours, then dry it. This is the pre-fired powder.

Benötigte Werkzeuge:

EisenkugelmühleEisenkugelmühle
Ethanol in Laborqualität, 95 %Ethanol in Laborqualität, 95 %
TrockenofenTrockenofen
5

Stir into 8 % polyvinyl acetate in acetone

Dissolve polyvinyl acetate in acetone to a 8 % solution and stir the pre-fired powder into it, 1 cc of solution per gram of powder. The binder burns off later.

Benötigte Werkzeuge:

PolyvinylacetatPolyvinylacetat
AcetonAceton
BalkenwaageBalkenwaage
6

Orient in a 10000 oersted field

Put the suspension in a moulding die between the poles of a magnet and apply a first field of 10000 oersted. Remove the binder solution while the field is on (as in Example 4).

Benötigte Werkzeuge:

Scheiben-PressformScheiben-Pressform
ElektromagnetElektromagnet
Hydraulische PresseHydraulische Presse
7

Heat to 500 °C without a field

Heat the blocks to 500 °C with no magnetic field.

Benötigte Werkzeuge:

RohrofenRohrofen
Hitzebeständige HandschuheHitzebeständige Handschuhe
8

Sinter: through a 1280 °C zone in 5 minutes

Pass the block at 20 mm per minute through an electric furnace in air at 1280 °C with a 10 cm hot zone: about 5 minutes in the heat.

Benötigte Werkzeuge:

RohrofenRohrofen
Hitzebeständige HandschuheHitzebeständige Handschuhe
9

Magnetise in the principal direction

Magnetise the block along the direction of the first field, the principal direction. The patent magnetises it in a field in that direction; ours: an electromagnet. Find the north face with a compass.

Benötigte Werkzeuge:

ElektromagnetElektromagnet
KompassKompass

Materialien

2

Benötigte Werkzeuge

15

Dieser Bauplan stellt her

Verwandte Blueprints

Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...