Strontium Ferrite Disc Magnet: Example 8 Without the Orienting Field (Gorter, Philips 1956, Ex. 8 Comparison)
Made as in Example 8 but without the first, orienting field. Gorter's comparison block held 2,020 gauss with a coercive force of 3,225 oersted and a (BH)max of 0.99 × 10⁶.
Source: E. W. Gorter, G. W. Rathenau and A. L. Stuyts (Philips), US 2,762,778 (1956), Example 8. They made blocks; disc size is ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Erfahren
3 days
Anweisungen
1
1
Weigh strontium carbonate and iron oxide
Weigh strontium carbonate and iron oxide
Weigh 29.5 g strontium carbonate and 179 g ferric oxide.
Materialien für diesen Schritt:
Strontiumcarbonat29.5 g
Eisen(III)-oxid179 gBenötigte Werkzeuge:
Balkenwaage
P100-Atemschutzmaske2
2
Mill 15 hours with alcohol, dry
Mill 15 hours with alcohol, dry
Grind in a ball mill with alcohol for 15 hours. Remove the alcohol and dry the powder.
Benötigte Werkzeuge:
Eisenkugelmühle
Ethanol in Laborqualität, 95 %
Trockenofen3
3
Pre-fire 2 hours at 1000 °C in air
Pre-fire 2 hours at 1000 °C in air
Heat the powder for 2 hours at 1000 °C in an electric furnace in air. Let it cool.
Benötigte Werkzeuge:
Muffelofen
Tiegel mit Deckel (Porzellan)
Tiegelzange
Hitzebeständige Handschuhe4
4
Grind 4 hours in an agate centrifugal mill
Grind 4 hours in an agate centrifugal mill
Grind the cooled material for 4 hours with alcohol in an agate centrifugal mill, then dry it. This is the pre-fired powder.
Benötigte Werkzeuge:
Achat-Zentrifugalmühle
Ethanol in Laborqualität, 95 %
Trockenofen5
5
Stir into 8 % polyvinyl acetate in acetone
Stir into 8 % polyvinyl acetate in acetone
Dissolve polyvinyl acetate in acetone to a 8 % solution and stir the pre-fired powder into it, 1 cc of solution per gram of powder. The binder burns off later.
Benötigte Werkzeuge:
Polyvinylacetat
Aceton
Balkenwaage6
6
Mould without a first field
Mould without a first field
Put the suspension in a moulding die and remove the binder solution without any magnetic field. This is the patent's comparison block.
Benötigte Werkzeuge:
Scheiben-Pressform
Hydraulische Presse7
7
Heat to 500 °C in a 2000 oersted field
Heat to 500 °C in a 2000 oersted field
Put the block in an electric furnace between the magnet's poles. With a second field of 2000 oersted along the first field's direction, heat to 500 °C, which burns off the rest of the binder. Then switch the field off.
Benötigte Werkzeuge:
Rohrofen
Elektromagnet
Hitzebeständige Handschuhe8
8
Sinter: through a 1280 °C zone in 5 minutes
Sinter: through a 1280 °C zone in 5 minutes
Pass the block at 20 mm per minute through an electric furnace in air at 1280 °C with a 10 cm hot zone: about 5 minutes in the heat.
Benötigte Werkzeuge:
Rohrofen
Hitzebeständige Handschuhe9
9
Magnetise the block
Magnetise the block
Magnetise the block in a field. Without the orienting field it has no preferred direction. Ours: an electromagnet. Find the north face with a compass.
Benötigte Werkzeuge:
Elektromagnet
KompassMaterialien
2- 29.5 gPlatzhalter
- 179 gPlatzhalter
Benötigte Werkzeuge
17- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
Dieser Bauplan stellt her
Verwandte Blueprints
Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien
CC0 Gemeinfrei
Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.
Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.