Potash Alum from Alum Shale
Charlie

Erstellt von

Charlie

11. Oktober 2026DE
27
0
0
0
0

Potash Alum from Alum Shale

Alum shale is a mix of iron pyrites, clay (aluminium silicate) and bituminous matter. Left to weather in the air, the pyrites oxidise and form sulphuric acid, which attacks the clay and turns it into aluminium sulphate. Water draws this out as a solution, which is settled, boiled down until iron sulphate crystallises out on cooling, then boiled down further to a specific gravity of 1.40. Stirred with the right amount of potassium sulphate, it throws down potash alum as a fine powder, alum meal. Alum crystallises in regular octahedra and is very soluble in water. Shale was also roasted to speed this up, which gives off sulphur dioxide; that route is not used here.
Erfahren
Weeks (weathering) plus days

Anweisungen

1

Weather the shale

Spread the broken shale in the open and let it weather, so the pyrites oxidise and the acid formed turns the clay into aluminium sulphate.

Materialien für diesen Schritt:

AlaunschieferAlaunschiefer1 as required
2

Extract

Wash the weathered mass with water, step by step, until the solution reaches a specific gravity of 1.16.

Materialien für diesen Schritt:

WasserWasser1 as required

Benötigte Werkzeuge:

Spindel (Aräometer)Spindel (Aräometer)
3

Settle

Let the solution stand so calcium sulphate and basic iron sulphate settle out, then draw it off.

Benötigte Werkzeuge:

AbsetzbeckenAbsetzbecken
4

Remove the iron

Boil it down until iron (ferrous) sulphate crystallises on cooling; draw off the liquor and boil it down to a specific gravity of 1.40.

Benötigte Werkzeuge:

SiedepfanneSiedepfanne
Spindel (Aräometer)Spindel (Aräometer)
5

Precipitate the alum

Let it stand, decant it from any sediment, add the calculated amount of potassium sulphate and stir well: the alum falls as a fine powder, alum meal. (With much iron present, potassium chloride is used instead.)

Materialien für diesen Schritt:

KaliumsulfatKaliumsulfat1 as required

Benötigte Werkzeuge:

AbsetzbeckenAbsetzbecken

Materialien

3
  • 1 as required
    Platzhalter
  • 1 as required
    Platzhalter
  • 1 as required
    Platzhalter

Benötigte Werkzeuge

3

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...