Samarium: Oxide Reduced with Graphite at 1700 °C in Vacuum and Distilled Twice (Downing, Gorski and Koerner, US 3,104,970)
Charlie

Erstellt von

Charlie

1. November 2026DE
5
0
0
0
0

Samarium: Oxide Reduced with Graphite at 1700 °C in Vacuum and Distilled Twice (Downing, Gorski and Koerner, US 3,104,970)

Samarium holds on to oxygen too hard for ordinary smelting. Heated with graphite in a hard vacuum it boils off as samarium carbide vapour; a second distillation of that carbide, caught on a tantalum plate, gives the metal itself. Result: samarium metal, 99.7 % pure. Source: J. H. Downing, H. L. Gorski and E. L. Koerner, US 3,104,970 (1963), Example I. Work at 1700 °C under vacuum. Picture drawn by Youblob.
Erfahren
1 day

Anweisungen

1

Mix and pellet

Mix intimately 79 parts by weight of 99.9 % samarium oxide with 21 parts of powdered graphite (12.7 % more carbon than the oxygen needs), with no particle larger than about 50 microns. Press into pellets 0.75 in across; pellets let the gases and vapour escape.

Materialien für diesen Schritt:

SamariumoxidSamariumoxid1 79 parts by weight

Benötigte Werkzeuge:

GraphitpulverGraphitpulver
Hydraulische PresseHydraulische Presse
2

Reduce and distil to carbide

Heat the pellets in a vacuum induction furnace to 1700 °C under 0.5 micron or less and hold three hours. Samarium carbide condenses on a graphite condenser (carbon resists the carbon monoxide given off). Only a little oxide and carbon stay behind; they can go back into the next charge.

Benötigte Werkzeuge:

GraphittiegelGraphittiegel
InduktionsofenInduktionsofen
VakuumpumpeVakuumpumpe
GraphitkondensatorGraphitkondensator
3

Distil the metal onto tantalum

Heat the carbide from the first condenser to 1700 °C under 0.05 micron and hold two hours. Samarium metal condenses on a tantalum condenser: 99.7 % samarium, 0.05 % carbon, 0.10 % oxygen.

Benötigte Werkzeuge:

GraphittiegelGraphittiegel
InduktionsofenInduktionsofen
VakuumpumpeVakuumpumpe
TantalkondensatorTantalkondensator

Materialien

1
  • 1 79 parts by weight
    Platzhalter

Benötigte Werkzeuge

7

Dieser Bauplan stellt her

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.