Screwdriver: a Flat Blade Forged, Packed at a Low Heat and Tempered Grey (Holford, 1907)
Forge

Erstellt von

Forge

4. November 2026NO
5
0
0
0
0

Screwdriver: a Flat Blade Forged, Packed at a Low Heat and Tempered Grey (Holford, 1907)

A flat screwdriver is a steel shank flattened to a blade that fits the slot of a screw. H. Holford's 20th Century Toolsmith and Steelworker (1907) says most smiths make them so they twist or break on a hard screw, and gives his cure: forge it from 75-point carbon steel, strike the blade a few good blows on each flat at a low heat, harden it and let the temper run to grey. His Fig. 60 shows the shape without its handle. He gives no sizes and no handle, which are unknown here; the brine bath is from his chapter on the hardening bath. Source: H. Holford (1907), pp. 21, 118. Picture: his Fig. 60.
Fortgeschritten
Half a day

Anweisungen

1

Read Holford

"Strike it a few good blows on each flat side of the screw driving edge while at a low heat. Then harden and allow the temper to draw to a grey, cool off and you will have a screw driver that will give unlimited satisfaction."
2

Forge the shape

Take good steel of 75 points carbon. Forge it to the shape of Fig. 60: a round shank, flattened at one end to the driving blade and drawn to a pointed tang at the other for the handle. Holford gives no sizes (unknown).

Materialien für diesen Schritt:

Werkzeugstahl-VierkantstabWerkzeugstahl-Vierkantstab1 bar

Benötigte Werkzeuge:

EsseEsse
AmbossAmboss
SchmiedehammerSchmiedehammer
SchmiedezangeSchmiedezange
Unbekannte MaßeUnbekannte Maße
SchutzbrilleSchutzbrille
Hitzebeständige HandschuheHitzebeständige Handschuhe
3

Pack the blade

At a low heat, strike a few good blows on each flat side of the driving edge.

Benötigte Werkzeuge:

SchmiedehammerSchmiedehammer
AmbossAmboss
EsseEsse
SchmiedezangeSchmiedezange
4

Harden and temper grey

Heat the blade end evenly and quench it in the hardening bath. Holford's bath is clean water free from grease, best made into a brine with as much salt as the water will dissolve, kept as large and as cold as possible. Brighten the blade with a file so the colours show, draw the temper to a grey, then cool it off.

Benötigte Werkzeuge:

EsseEsse
Gesättigte SalzlakeGesättigte Salzlake
SchmiedezangeSchmiedezange
Feine FeileFeine Feile
Hitzebeständige HandschuheHitzebeständige Handschuhe
5

Fit a handle

Fit a handle on the tang. Holford shows the screwdriver without one and does not say what it is made of (unknown).

Materialien für diesen Schritt:

Unbekanntes MaterialUnbekanntes Material1 handle
6

History and honest limits

Holford, a toolsmith writing for blacksmiths and tool dressers, says a good screwdriver is prized by every mechanic, woodworkers most of all, yet few smiths could make one that would not break or twist. His temper table lists the screwdriver at grey, in 0.75 carbon steel. He gives no sizes, no handle and no heat for hardening; those are unknown here, and the tools are ours.

Materialien

2

Benötigte Werkzeuge

9

Verwandte Blueprints

Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...