Semi-Cured Phenolic Sheet: Paper Dipped in Phenol Resin and Part-Cured at 120-130 °C (Lucas, Western Electric, US 1,470,990)
Charlie

Erstellt von

Charlie

31. Oktober 2026DE
1
0
0
0
0

Semi-Cured Phenolic Sheet: Paper Dipped in Phenol Resin and Part-Cured at 120-130 °C (Lucas, Western Electric, US 1,470,990)

Paper soaked in phenol resin is dried, then cured only part of the way, so the resin is stiff but not yet hard. Lucas did this before the final hot press so the press would not squeeze the resin out of the fibres. Result: a dry, partly cured phenolic sheet that a later coat of phenolic resin can still bond into. Source: Lucas, US 1,470,990 (Western Electric, 1923). Stopping before his final hot press is ours. Not given: the solvent in his resin, paper grade, mercerising strengths. Picture drawn by Youblob.
Fortgeschritten
1 hour

Anweisungen

1

Dip the paper in phenol resin

Run the paper through a bath of phenol resin of specific gravity about 0.970: about 2 minutes for plain paper, 1 minute or less if mercerised first. Ours: Liquid Bakelite as the resin; Lucas does not say how it was thinned.

Materialien für diesen Schritt:

PapierPapier1 as required
Flüssiges Bakelit (Phenol-Formaldehyd-Kondensationsprodukt)Flüssiges Bakelit (Phenol-Formaldehyd-Kondensationsprodukt)1 as required

Benötigte Werkzeuge:

Prepreg-ImprägnieranlagePrepreg-Imprägnieranlage
Spindel (Aräometer)Spindel (Aräometer)
2

Optional: mercerise the paper first

For faster, fuller soaking, first pass the paper through caustic soda, squeeze, wash in water, neutralise in an acid, wash again and dry. Strengths and the acid: not given.

Benötigte Werkzeuge:

Ätznatron (Natriumhydroxid)Ätznatron (Natriumhydroxid)
Prepreg-ImprägnieranlagePrepreg-Imprägnieranlage
3

Dry at about 90 °C

Dry the soaked paper in an oven at about 90 °C, just long enough to dry it.

Benötigte Werkzeuge:

TrockenofenTrockenofen
4

Part-cure at 120-130 °C

Pass the dry paper through a curing oven at 120-130 °C for about 10 minutes (Lucas's description; his claim 4 says 125 °C for about 10 seconds). The resin sets as stiff as the fibres, but does not harden through.

Benötigte Werkzeuge:

AushärteofenAushärteofen
5

Dip again for 10-15 seconds and dry

Dip the part-cured paper in phenol resin again for 10-15 seconds, then dry at about 90 °C until it can be wound on a reel. Stop here: the sheet is semi-cured. Lucas's next step, stacking and hot pressing, cures it fully.

Materialien für diesen Schritt:

Flüssiges Bakelit (Phenol-Formaldehyd-Kondensationsprodukt)Flüssiges Bakelit (Phenol-Formaldehyd-Kondensationsprodukt)1 as required

Benötigte Werkzeuge:

Prepreg-ImprägnieranlagePrepreg-Imprägnieranlage
TrockenofenTrockenofen

Materialien

2

Benötigte Werkzeuge

5

Verwandte Blueprints

Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...