Silver Oxide: Silver Nitrate Precipitated with Solution of Potassa (USP 1870)
Silver oxide is a heavy, dark brown powder, and heating it to about 250 °C leaves pure silver. Potash added to a silver nitrate solution throws it down, and washing leaves potassium nitrate behind in the water.
Source: US Pharmacopoeia 1870, as quoted in the US Dispensatory (1907), Argenti Oxidum. Not given here: the strength of the solution of potassa; ours: potassium hydroxide in distilled water. Silver nitrate stains and burns skin: gloves and goggles. Picture drawn by Youblob.
Anfänger
1 day
Anweisungen
1
1
Dissolve 4 troy oz silver nitrate in half a pint of water
Dissolve 4 troy oz silver nitrate in half a pint of water
Dissolve 4 troy ounces of silver nitrate in half a pint of distilled water. Silver nitrate stains and burns skin: gloves and goggles.
Materialien für diesen Schritt:
Silbernitrat4 troy oz
Destilliertes Wasser0.5 pintBenötigte Werkzeuge:
Balkenwaage
Becherglas aus Borosilikat
Borosilikatglasstab
Nitrilhandschuhe
Chemikalienschutzbrille2
2
Add solution of potassa while it still precipitates
Add solution of potassa while it still precipitates
Add solution of potassa, about a pint and a half or as much as needed, for as long as it still throws down a precipitate. Ours: potassium hydroxide dissolved in distilled water; the USP strength is not given here. Potash free of carbon dioxide keeps out silver carbonate.
Materialien für diesen Schritt:
Kaliumhydroxid1 as required
Destilliertes Wasser1.5 pintBenötigte Werkzeuge:
Becherglas aus Borosilikat
Borosilikatglasstab
Nitrilhandschuhe
Chemikalienschutzbrille3
3
Wash, dry and store in the dark
Wash, dry and store in the dark
Wash the precipitate again and again with water until the washings are almost tasteless. Dry it and keep it in a well-stoppered bottle away from light. Ours: filter paper, and a low oven, well below the 250 °C at which it breaks down to silver.
Benötigte Werkzeuge:
Filterpapier
Destilliertes Wasser
Trockenofen
Dunkelglasgefäße mit luftdichtem VerschlussMaterialien
3- 4 troy ozPlatzhalter
- 2 pintPlatzhalter
- 1 as requiredPlatzhalter
Benötigte Werkzeuge
9- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
Dieser Bauplan stellt her
Verwandte Blueprints
Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien
CC0 Gemeinfrei
Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.
Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.