Neodymium Magnets, Sample 12: 55Fe-30B-15Nd Sintered (Sagawa 1988)
Neodymium magnets are iron, boron and neodymium. Sagawa's team at Sumitomo melted the three together, ground the casting to a powder finer than 10 µm, lined the grains up in a magnetic field while pressing them, and sintered the compact in argon. This is their sample 12, 55 % iron, 30 % boron and 15 % neodymium by atoms: 4.0 MGOe.
Source: M. Sagawa et al. (Sumitomo Special Metals), US 4,770,723 (1988). Unknown: how the pure iron, the ferroboron and the neodymium metal are made, and how the finished magnets are magnetised; the patent does not say. The 1 kg weights are our arithmetic from the patent's atomic percentages. Picture: the patent's Fig. 8.
Experte
2 days
Anweisungen
1
1
Weigh sample 12: 55 Fe, 30 B, 15 Nd
Weigh sample 12: 55 Fe, 30 B, 15 Nd
Sample 12 is 55 % iron, 30 % boron and 15 % neodymium by atoms. Use 99.9 % electrolytic iron, ferroboron (19.38 % B, 5.32 % Al, 0.74 % Si, 0.03 % C, the rest iron) and neodymium of 99.7 % or better. Ours: a 1 kg melt, by arithmetic: 328.1 g iron, 301.0 g ferroboron, 389.2 g neodymium. Unknown: how these three are made.
Materialien für diesen Schritt:
Elektrolyteisen328.1 g
Ferrobor301 g
Neodym-Metall389.2 gBenötigte Werkzeuge:
Balkenwaage2
2
Melt by high frequency in argon and cast
Melt by high frequency in argon and cast
Melt the charge in a high-frequency (induction) furnace under argon and pour it into a water-cooled copper mould.
Benötigte Werkzeuge:
Induktionsofen
Schmelztiegel aus Schamotte
Argon
Druckgasflasche
Wassergekühlte Kupferform
Hitzebeständige Handschuhe3
3
Stamp to 35 mesh, ball-mill to 3-10 µm
Stamp to 35 mesh, ball-mill to 3-10 µm
Crush the casting in a stamp mill until it passes a 35-mesh sieve. Then grind it in a ball mill for 3 hours, to 3-10 µm.
Benötigte Werkzeuge:
Pochwerk
Siebsatz (abgestufte Maschenweiten)
Eisenkugelmühle
Schutzbrille4
4
Press in a 10 kOe field at 1.5 t/cm²
Press in a 10 kOe field at 1.5 t/cm²
Line the powder up in a magnetic field of 10 kOe and press it at 1.5 tonnes per cm². Unknown: the size and shape of the magnets.
Benötigte Werkzeuge:
Magnetfeldpresse5
5
Sinter in argon at 1000-1200 °C
Sinter in argon at 1000-1200 °C
Sinter the compacts at 1000-1200 °C for about one hour in argon, then let them cool. Sample 12 measured 4.2 kG remanence, 10.7 kOe coercivity and 4.0 MGOe.
Benötigte Werkzeuge:
Rohrofen
Argon
Druckgasflasche
Hitzebeständige Handschuhe6
6
Magnetise the magnets
Magnetise the magnets
Unknown: how the sintered magnets are magnetised. Sagawa measures them on a B-H tracer but gives no magnetising field or apparatus.
Benötigte Werkzeuge:
Unbekanntes MagnetisierverfahrenMaterialien
3- 328.1 gPlatzhalter
- 301 gPlatzhalter
- 389.2 gPlatzhalter
Benötigte Werkzeuge
14- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
Dieser Bauplan stellt her
Verwandte Blueprints
Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien
CC0 Gemeinfrei
Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.
Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.