Neodymium Magnets, Sample 7: 77Fe-8B-15Nd Sintered (Sagawa 1988)
Forge

Erstellt von

Forge

28. Oktober 2026NO
3
0
0
0
0

Neodymium Magnets, Sample 7: 77Fe-8B-15Nd Sintered (Sagawa 1988)

Neodymium magnets are iron, boron and neodymium. Sagawa's team at Sumitomo melted the three together, ground the casting to a powder finer than 10 µm, lined the grains up in a magnetic field while pressing them, and sintered the compact in argon. This is their sample 7, 77 % iron, 8 % boron and 15 % neodymium by atoms: 32.1 MGOe. Source: M. Sagawa et al. (Sumitomo Special Metals), US 4,770,723 (1988). Unknown: how the pure iron, the ferroboron and the neodymium metal are made, and how the finished magnets are magnetised; the patent does not say. The 1 kg weights are our arithmetic from the patent's atomic percentages. Picture: the patent's Fig. 8.
Experte
2 days

Anweisungen

1

Weigh sample 7: 77 Fe, 8 B, 15 Nd

Sample 7 is 77 % iron, 8 % boron and 15 % neodymium by atoms. Use 99.9 % electrolytic iron, ferroboron (19.38 % B, 5.32 % Al, 0.74 % Si, 0.03 % C, the rest iron) and neodymium of 99.7 % or better. Ours: a 1 kg melt, by arithmetic: 605.7 g iron, 68.1 g ferroboron, 330.3 g neodymium. Unknown: how these three are made.

Materialien für diesen Schritt:

ElektrolyteisenElektrolyteisen605.7 g
FerroborFerrobor68.1 g
Neodym-MetallNeodym-Metall330.3 g

Benötigte Werkzeuge:

BalkenwaageBalkenwaage
2

Melt by high frequency in argon and cast

Melt the charge in a high-frequency (induction) furnace under argon and pour it into a water-cooled copper mould.

Benötigte Werkzeuge:

InduktionsofenInduktionsofen
Schmelztiegel aus SchamotteSchmelztiegel aus Schamotte
ArgonArgon
DruckgasflascheDruckgasflasche
Wassergekühlte KupferformWassergekühlte Kupferform
Hitzebeständige HandschuheHitzebeständige Handschuhe
3

Stamp to 35 mesh, ball-mill to 3-10 µm

Crush the casting in a stamp mill until it passes a 35-mesh sieve. Then grind it in a ball mill for 3 hours, to 3-10 µm.

Benötigte Werkzeuge:

PochwerkPochwerk
Siebsatz (abgestufte Maschenweiten)Siebsatz (abgestufte Maschenweiten)
EisenkugelmühleEisenkugelmühle
SchutzbrilleSchutzbrille
4

Press in a 10 kOe field at 1.5 t/cm²

Line the powder up in a magnetic field of 10 kOe and press it at 1.5 tonnes per cm². Unknown: the size and shape of the magnets.

Benötigte Werkzeuge:

MagnetfeldpresseMagnetfeldpresse
5

Sinter in argon at 1000-1200 °C

Sinter the compacts at 1000-1200 °C for about one hour in argon, then let them cool. Sample 7 measured 12.1 kG remanence, 7.3 kOe coercivity and 32.1 MGOe.

Benötigte Werkzeuge:

RohrofenRohrofen
ArgonArgon
DruckgasflascheDruckgasflasche
Hitzebeständige HandschuheHitzebeständige Handschuhe
6

Magnetise the magnets

Unknown: how the sintered magnets are magnetised. Sagawa measures them on a B-H tracer but gives no magnetising field or apparatus.

Benötigte Werkzeuge:

Unbekanntes MagnetisierverfahrenUnbekanntes Magnetisierverfahren

Materialien

3

Benötigte Werkzeuge

14

Verwandte Blueprints

Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...