Strontium Ferrite Disc Magnet, Sintered 4 Hours at 1200 °C (Went, Philips 1956, Ex. 34)
Charlie

Erstellt von

Charlie

28. Oktober 2026DE
2
0
0
0
0

Strontium Ferrite Disc Magnet, Sintered 4 Hours at 1200 °C (Went, Philips 1956, Ex. 34)

A strontium ferrite magnet made exactly like Went's barium ferrite of Example 34, with strontium carbonate in place of barium carbonate: 29.5 g of it to 191.7 g iron oxide, milled, fired, milled again, pressed and sintered for 4 hours. This iteration sinters at 1200 °C, where his rod held 1,340 gauss with a coercive force of 3,900 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 34. They pressed rods; the disc size is ours. The patent does not say how to magnetise it; our way is stated. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Erfahren
2 days

Anweisungen

1

Weigh strontium carbonate and iron oxide

Weigh 29.5 g of strontium carbonate and 191.7 g of ferric oxide, Fe2O3. The patent makes this second mixture "in exactly the same manner" as the barium one.

Materialien für diesen Schritt:

StrontiumcarbonatStrontiumcarbonat29.5 g
Eisen(III)-oxidEisen(III)-oxid191.7 g

Benötigte Werkzeuge:

BalkenwaageBalkenwaage
GummihandschuheGummihandschuhe
P100-AtemschutzmaskeP100-Atemschutzmaske
2

Mill with ethanol for 4 hours

Grind the mixture with ethanol in an iron ball mill for 4 hours. Let the ethanol evaporate, then dry the powder in a drying oven.

Benötigte Werkzeuge:

EisenkugelmühleEisenkugelmühle
Ethanol in Laborqualität, 95 %Ethanol in Laborqualität, 95 %
TrockenofenTrockenofen
3

Presinter at 1000 °C for 4 hours

Fire the dry powder in air at 1000 °C for 4 hours (ours: in a lidded porcelain crucible in a muffle furnace). Let it cool.

Benötigte Werkzeuge:

MuffelofenMuffelofen
Tiegel mit Deckel (Porzellan)Tiegel mit Deckel (Porzellan)
TiegelzangeTiegelzange
Hitzebeständige HandschuheHitzebeständige Handschuhe
4

Mill again for 4 hours

Grind the presintered product with ethanol in the ball mill for another 4 hours. Let the ethanol evaporate.

Benötigte Werkzeuge:

EisenkugelmühleEisenkugelmühle
Ethanol in Laborqualität, 95 %Ethanol in Laborqualität, 95 %
TrockenofenTrockenofen
P100-AtemschutzmaskeP100-Atemschutzmaske
5

Press discs at 1.5 tons per cm²

Press the powder at 1.5 tons/cm². The patent pressed rods; we press discs. Ours: a die 20 mm across, so about 4.7 tonnes on the punch (our arithmetic: 1.5 × 3.14 cm²).

Benötigte Werkzeuge:

Hydraulische PresseHydraulische Presse
Scheiben-PressformScheiben-Pressform
6

Sinter 4 hours at 1200 °C

Sinter the discs for 4 hours at 1200 °C in oxygen or in air. The patent's strontium rod at 1200 °C: 1,340 gauss and 3,900 oersted.

Benötigte Werkzeuge:

MuffelofenMuffelofen
TiegelzangeTiegelzange
Hitzebeständige HandschuheHitzebeständige Handschuhe
7

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Benötigte Werkzeuge:

ElektromagnetElektromagnet
KompassKompass

Materialien

2

Benötigte Werkzeuge

14

Dieser Bauplan stellt her

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.