Teaspoon Forged from a Silver Bar (Payne 1914)
Arthur F. Payne · Public domain (1914)
Forge

Erstellt von

Forge

27. Oktober 2026NO
13
0
0
0
0

Teaspoon Forged from a Silver Bar (Payne 1914)

A 6-inch silver teaspoon forged out of a small bar of silver, the way a blacksmith forges iron. Arthur Payne called it the hardest of his five spoon methods, but the cheapest, because almost no silver is wasted. Source: A. F. Payne, Art Metalwork with Inexpensive Equipment (1914), pp. 184–186; annealing from his chapter XI. Cutting the bar from sheet is ours. Picture: Payne's Fig. 158, teaspoons forged this way.
Erfahren
1 day

Anweisungen

1

Cut the silver bar

For a teaspoon 6 in long you need a piece of sterling silver 4 in long, ½ in wide and ⅛ in thick. Mark it out and saw it from sheet of that thickness (cutting from sheet is ours).

Materialien für diesen Schritt:

Blech aus SterlingsilberBlech aus Sterlingsilber1 piece 4 × ½ × ⅛ in

Benötigte Werkzeuge:

ReißnadelReißnadel
JuweliersägeJuweliersäge
2

Forge out the bowl

Heat the bar until it is almost red-hot, hold it in tongs and forge the bowl out on the anvil. Silver forges more easily when it is nearly red, but never hammer it while it is red-hot: it will crack.

Benötigte Werkzeuge:

BunsenbrennerBunsenbrenner
ZangeZange
AmbossAmboss
HammerHammer
3

Work bowl, then shank and handle

Hammer the bowl until it is hard, then the shank and handle, so the whole spoon is hard before you anneal it again. That saves time.

Benötigte Werkzeuge:

AmbossAmboss
HammerHammer
4

Anneal and repeat

To soften it, heat it to a dull red and plunge it into water, or let it cool. Then go on forging until the spoon is roughly to shape.

Materialien für diesen Schritt:

WasserWasser1 as required

Benötigte Werkzeuge:

BunsenbrennerBunsenbrenner
ZangeZange
GlasgefäßGlasgefäß
5

Trim with shears and file

Trim the outline with the shears and file the edges smooth.

Benötigte Werkzeuge:

KraftblechschereKraftblechschere
Feilen (Handfeile)Feilen (Handfeile)
6

Polish out the file marks

Rub out all the scratches and file marks with emery cloth.

Benötigte Werkzeuge:

SchmirgelleinenSchmirgelleinen
7

Anneal to even the fire scale

Anneal the spoon thoroughly once more. Heated silver grows a thin white skin, the fire scale, and this brings it back over the spots where filing and polishing took it off, so the colour is even.

Materialien für diesen Schritt:

WasserWasser1 as required

Benötigte Werkzeuge:

BunsenbrennerBunsenbrenner
ZangeZange
GlasgefäßGlasgefäß
8

Planish with smooth hammers

Planish the spoon on smooth tools with smooth, bright hammers. This makes it stiff again after the annealing.

Benötigte Werkzeuge:

PlanierhammerPlanierhammer
AmbossAmboss
PflockPflock
9

Final polish with rouge

Polish it lightly with a soft cotton flannel and a little red rouge.

Benötigte Werkzeuge:

SchmuckpoliertuchSchmuckpoliertuch
PolierrotPolierrot

Materialien

2

Benötigte Werkzeuge

14

Dieser Bauplan stellt her

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...