Thread Locker: Tetraethylene Glycol Dimethacrylate with Cumene Hydroperoxide, Set When Air Is Shut Out (Krieble, US 2,895,950)
An anaerobic thread locker. A little cumene hydroperoxide stirred into tetraethylene glycol dimethacrylate stays liquid as long as air reaches it. Shut between threads or plates, away from air, it sets into a tough resin and locks them.
Result: a liquid that keeps a year or more in a half-full bottle and locks steel in 40 minutes to 5 hours, depending on how much catalyst it holds. Heat speeds it up.
Source: V. K. Krieble (American Sealants Company), US 2,895,950 (1959), Example 1. Unknown: how the tetraethylene glycol dimethacrylate is made; the patent uses a bought commercial grade. Not given: bond strength. Picture: Wikimedia Commons.
Anfänger
2 hours
Anweisungen
1
1
Mix in the catalyst
Mix in the catalyst
At room temperature, stir cumene hydroperoxide into commercial-grade tetraethylene glycol dimethacrylate, measuring by volume. Anything from 0.1 to 10 % works; the patent prefers 2 to 10 %. Goggles and gloves: cumene hydroperoxide is an organic peroxide, keep it cool.
Materialien für diesen Schritt:
Tetraethylenglykoldimethacrylat100 parts by volume
Cumolhydroperoxid5 parts by volume (0.1-10)Benötigte Werkzeuge:
Messzylinder
Rührstab
Vollsichtschutzbrille
Chemikalienbeständige Handschuhe2
2
Store it with air
Store it with air
Keep the mixture in a container with air space, preferably polyethylene, which lets air through. Bottles stored half full stayed liquid for a year or more at room temperature.
Benötigte Werkzeuge:
Kunststoffflasche3
3
Apply to the threads
Apply to the threads
Put a few drops on the threads before joining the parts. Once air is shut out it sets. Average set times between steel plates at 25-27 °C, by catalyst share: 10 %, 42 min; 5 %, 52 min; 2 1/2 %, 74 min; 1 1/4 %, 84 min. With 0.1 % it takes about five hours.
Benötigte Werkzeuge:
Pipetten- und Tropferset4
4
Speed it up with heat
Speed it up with heat
Heat sets it faster: the 0.1 % mixture between glass slides, warmed to 100 °C over a steam bath, locked them in five minutes. Ours: a water bath over a burner as the steam bath.
Benötigte Werkzeuge:
Wasserbad
BunsenbrennerMaterialien
2- 100 parts by volumePlatzhalter
- 5 parts by volume (0.1-10)Platzhalter
Benötigte Werkzeuge
8- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
Dieser Bauplan stellt her
Verwandte Blueprints
Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien
CC0 Gemeinfrei
Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.
Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.