Tin Oxide: Tin Burnt in an Open Iron Pot
Charlie

Erstellt von

Charlie

14. Oktober 2026DE
15
0
0
0
0

Tin Oxide: Tin Burnt in an Open Iron Pot

Tin oxide is made by burning tin in air: melted tin in an open pot slowly turns to a white powder. Andrew Ure (1839) describes the enamel makers' way, with a lead-tin alloy in a flat iron pot, the powder raked aside as it forms, then ground and washed fine. Done with pure tin it gives the milky white oxide used in glazes, opal glass and polishing. The picture: tin(IV) oxide powder on a watch glass.
Fortgeschritten
A day

Anweisungen

1

Melt the tin in an open pot

Melt the tin in a flat cast-iron pot over a charcoal fire. Leave the pot open to the air.

Materialien für diesen Schritt:

ZinnbarrenZinnbarren1 kg
HolzkohleHolzkohle1 as required

Benötigte Werkzeuge:

BalkenwaageBalkenwaage
Gusseiserner SchmelztiegelGusseiserner Schmelztiegel
Holzkohle-TiegelofenHolzkohle-Tiegelofen
ZangeZange
Hitzebeständige HandschuheHitzebeständige Handschuhe
2

Burn it, rake the powder aside

Raise the heat towards a dull red and keep stirring the surface. Rake the white crust to the sides as it forms, as Ure describes, and add tin as it is used up. Keep the heat as low as will do: Ure warns that too strong a fire fuses the powder and makes it hard to grind.

Benötigte Werkzeuge:

Gusseiserner SchmelztiegelGusseiserner Schmelztiegel
EisenrechenEisenrechen
LochkelleLochkelle
Hitzebeständige HandschuheHitzebeständige Handschuhe
3

Pick out the metal

Let the powder cool. Sift it and pick out any beads of tin; Ure: no metal may be left in the oxide. Melt the beads back in.

Benötigte Werkzeuge:

FeinsiebFeinsieb
ChemikalienschutzbrilleChemikalienschutzbrille
4

Grind and wash

Grind the powder fine with water. Stir it up in a bucket of water, let the coarse part settle for a moment and pour off the milky water; let the fine part settle out of that, as Ure washed his. Dry it in a dish and store it closed.

Materialien für diesen Schritt:

WasserWasser10 Liter

Benötigte Werkzeuge:

Mörser und PistillMörser und Pistill
LäuferLäufer
EimerEimer
AbdampfschaleAbdampfschale
EinmachglasEinmachglas
5

Tin to oxide

Jupyter-Notebook wird geladen …
6

Limits

Burning tin in air is how tin oxide is made (Wikipedia); the pot, raking, low heat and washing are Ure's practice for the lead-tin calx of enamel makers, used here with pure tin by our choice. Tin oxidises more slowly than Ure's lead-rich alloy, so allow time.

Materialien

3
  • Platzhalter
  • 1 as required
    Platzhalter
  • 10 Liter
    Platzhalter

Benötigte Werkzeuge

14

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...