Guitar Strings: Bronze Wound on Steel, Then Heat-Soaked (Stone and Falcone 1977)

A wound string is a steel core with another wire wrapped round it. Stone and Falcone believed the wrap keeps stresses from the winding and slowly unwinds as the string is played, so the tone goes dead. Their fix: after winding, heat-soak the string, at least 2 hours at 270 °F or 30 minutes at 480 °F for a bronze wrap, then let it cool. Source: W. N. Stone and A. S. Falcone (National Musical String Co.), US 4,063,674 (1977). Unknown: the winding itself (the patent calls it conventional), where phosphor bronze wire comes from, and the gauges. These are linked to unknown heads. The plain strings of the set are steel music wire; that, the oven and the nitrogen are ours. Picture drawn by Youblob.
Erfahren
1 day

Anweisungen

1

Cut the core and plain strings

Cut steel music wire for the cores of the wound strings and for the plain strings of the set. Unknown: the gauges and lengths, and the ball ends.

Materialien für diesen Schritt:

Federstahldraht 0,032 ZollFederstahldraht 0,032 Zoll1 as required

Benötigte Werkzeuge:

SeitenschneiderSeitenschneider
Unbekannte MaßeUnbekannte Maße
2

Wind the bronze wrap at room temperature

Wrap phosphor bronze wire helically round each core at room temperature. The patent prefers a wrap that expands more with heat than the core. Unknown: how; the patent says only 'in a conventional manner'.

Materialien für diesen Schritt:

PhosphorbronzedrahtPhosphorbronzedraht1 as required

Benötigte Werkzeuge:

Unbekanntes WickelverfahrenUnbekanntes Wickelverfahren
Unbekannte MaßeUnbekannte Maße
SchutzbrilleSchutzbrille
3

Heat-soak the wound strings

Heat the wound strings for a bronze wrap at 270-480 °F (132-249 °C): at least 2 hours at 270 °F or at least 30 minutes at 480 °F, shorter the hotter. If the wire tarnishes in hot air, do it without air, in nitrogen or carbon dioxide. The wrap's turns settle into more even spacing.

Benötigte Werkzeuge:

BackofenBackofen
LaborthermometerLaborthermometer
StickstoffflascheStickstoffflasche
4

Cool and set up the set

Let the strings cool back to room temperature. Make up the set with the plain steel strings.

Benötigte Werkzeuge:

SeitenschneiderSeitenschneider

Materialien

2

Benötigte Werkzeuge

7

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...