Metal Oxide Varistor: Zinc Oxide with 0.05 % Bismuth Oxide, 1100 °C, 1.0 mm (Masuyama 1972)
Ed

Erstellt von

Ed

28. Oktober 2026FI
3
0
0
0
0

Metal Oxide Varistor: Zinc Oxide with 0.05 % Bismuth Oxide, 1100 °C, 1.0 mm (Masuyama 1972)

A non-linear resistor: the current through it rises far faster than the voltage across it. Masuyama, Matsuoka and Nishi made one from zinc oxide with a little bismuth oxide: pressed into a disc, sintered, lapped, and given metal electrodes. With 0.05 mole % bismuth oxide, sintered at 1100 °C and lapped to 1.0 mm, the disc measured a C-value of 30 at 1 mA and a nonlinearity exponent n of 3.0. Source: T. Masuyama, M. Matsuoka and T. Nishi (Matsushita), US 3,663,458 (1972), Example 1. Unknown: how the aluminium is sprayed on and what the silver paint is. The patent calls both well known, so they are linked to unknown heads. The 10 g batch is our arithmetic. Picture: the patent's drawing.
Erfahren
1 day

Anweisungen

1

Weigh 99.95 : 0.05 and wet-mill 5 hours

Mix zinc oxide and bismuth oxide 99.95 : 0.05 by moles. Ours, for 10 g: 9.971 g zinc oxide, 0.029 g bismuth oxide (our arithmetic). Mill wet for 5 hours, then dry. Unknown: the milling liquid.

Materialien für diesen Schritt:

ZinkoxidpulverZinkoxidpulver9.971 g
BismutoxidBismutoxid0.029 g

Benötigte Werkzeuge:

BalkenwaageBalkenwaage
EisenkugelmühleEisenkugelmühle
TrockenofenTrockenofen
2

Press discs 13 mm by 2.5 mm

Press the powder in a mould into discs 13 mm across and 2.5 mm thick at 340 kg/cm².

Benötigte Werkzeuge:

Hydraulische PresseHydraulische Presse
Scheiben-PressformScheiben-Pressform
MessschieberMessschieber
3

Sinter 1 hour at 1100 °C and furnace-cool

Sinter the discs in air for 1 hour at 1100 °C, then let them cool in the furnace to room temperature (about 15-30 °C).

Benötigte Werkzeuge:

MuffelofenMuffelofen
4

Lap both faces to 1.0 mm

Lap both faces with 600-mesh silicon carbide until the disc is 1.0 mm thick.

Benötigte Werkzeuge:

Siliciumcarbid-KörnungSiliciumcarbid-Körnung
MessschieberMessschieber
5

Spray aluminium electrodes and attach leads

Spray a metallised film of aluminium on both faces. Attach a lead wire to each with conductive silver paint. Unknown: the spraying method and the paint.

Materialien für diesen Schritt:

AluminiumbarrenAluminiumbarren1 as required
SilberleitlackSilberleitlack1 as required
KupferdrahtKupferdraht2 Stück

Benötigte Werkzeuge:

Unbekanntes MetallspritzverfahrenUnbekanntes Metallspritzverfahren
MessschieberMessschieber

Materialien

5

Benötigte Werkzeuge

9

Verwandte Blueprints

Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...