Metal Oxide Varistor: Pure Zinc Oxide at 1000 °C, Bismuth Oxide Paste Fired at 800 °C (Masuyama 1972, Ex. 4)
A varistor made the other way round: a disc of pure zinc oxide, sintered, with bismuth oxide fired into its faces from a paste instead of mixed in. Sintered at 1000 °C and fired with the paste at 800 °C, the disc measured a C-value of 230 at 1 mA and a nonlinearity exponent n of 8.3. Masuyama found that firing on the bismuth oxide paste raises n a great deal over mixing it in.
Source: T. Masuyama, M. Matsuoka and T. Nishi (Matsushita), US 3,663,458 (1972), Example 4. Unknown: how the aluminium is sprayed on, what the silver paint is, and how strong the epoxy solution of the paste is. The 10 g batch is our arithmetic. Picture: the patent's drawing.
Erfahren
2 days
Anweisungen
1
1
Press pure zinc oxide at 340 kg/cm²
Press pure zinc oxide at 340 kg/cm²
Press zinc oxide powder at 340 kg/cm². Example 4 gives no disc size; ours: discs 13 mm across and 2.5 mm thick in the mould of Example 1.
Materialien für diesen Schritt:
Zinkoxidpulver1 as requiredBenötigte Werkzeuge:
Balkenwaage
Hydraulische Presse
Scheiben-Pressform
Messschieber2
2
Sinter 1 hour at 1000 °C and cool
Sinter 1 hour at 1000 °C and cool
Heat the pressed disc for 1 hour at 1000 °C, then let it cool to room temperature.
Benötigte Werkzeuge:
Muffelofen3
3
Lap both faces
Lap both faces
Lap both faces with silicon carbide abrasive. Example 4 gives no thickness.
Benötigte Werkzeuge:
Messschieber4
4
Coat with bismuth oxide paste and fire at 800 °C
Coat with bismuth oxide paste and fire at 800 °C
Coat both lapped faces with a paste of 50 % by weight bismuth oxide in a solution of epoxy resin in butyl alcohol, and fire it in air at 800 °C for 30 minutes. The bismuth oxide diffuses into the zinc oxide. Not given: how much paste, or the strength of the epoxy solution.
Materialien für diesen Schritt:
Bismutoxid1 as requiredBenötigte Werkzeuge:
Epoxidharz
n-Butanol
Muffelofen5
5
Spray aluminium electrodes and attach leads
Spray aluminium electrodes and attach leads
Spray a metallised film of aluminium on both faces. Attach a lead wire to each with conductive silver paint, as in Example 1. Unknown: the spraying method and the paint.
Materialien für diesen Schritt:
Aluminiumbarren1 as required
Silberleitlack1 as required
Kupferdraht2 StückBenötigte Werkzeuge:
Unbekanntes Metallspritzverfahren
MessschieberMaterialien
5- 1 as requiredPlatzhalter
- 1 as requiredPlatzhalter
- 1 as requiredPlatzhalter
- 1 as requiredPlatzhalter
- 2 StückPlatzhalter
Benötigte Werkzeuge
9- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
- Platzhalter
Dieser Bauplan stellt her
Verwandte Blueprints
Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien